Preparation method and application of perylene metal compound and composite material thereof
By using perylene-3,4,9,10-tetracarboxylic dianhydride and metal organic compounds in the catalyst to form perylene-type metal compounds and their composite materials with porous structures, the photocatalyst carrier kinetics and Thermodynamic problems improve NO oxidation efficiency and avoid the generation of by-products, achieving efficient and environmentally friendly NO removal effect.
Patent Information
- Application Number
- CN202211254630.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-10-13
AI Technical Summary
During the catalytic NO oxidation process, existing photocatalysts are easy to recombinate carriers, have poor visible light absorption, and may produce toxic by-products, affecting the catalytic effect, and it is difficult to meet the needs of efficient NO removal.
Perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) and metal organic compounds (such as tetrabutyl titanate) are used to mix ultrasonically in aqueous NaOH solution, and perylene metals are synthesized by microwave or hydrothermal method. The compounds and their composite materials form porous structures and two-dimensional layered structures, enhancing catalytic activity and selectivity.
The conversion rate of NO oxidation is improved, the generation of toxic by-products is avoided, visible light absorption is enhanced, and efficient NO removal is achieved, while ensuring environmental protection and low energy consumption in the preparation process.
Smart Images

Figure CN115611915B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic synthesis, and in particular relates to a preparation method and application of a perylene metal compound and a composite material thereof. Background Art
[0002] In recent years, the emission of automobile exhaust and the combustion of fossil fuels have led to a continuous increase in the content of nitrogen oxides in the atmosphere, which in turn has caused a series of environmental problems such as photochemical smog and ozone layer depletion, which seriously endanger human life and health. Therefore, it is necessary to find an effective nitrogen oxide removal technology. At present, traditional nitrogen oxide removal methods include selective catalytic reduction and selective non-catalytic reduction technology, which have good effects on the removal of high-concentration NOx, but the concentration of NO after treatment fails to meet human health standards. Photocatalytic NO oxidation, as a low-concentration NO removal technology, has the characteristics of low energy consumption, green and pollution-free, and low economic cost. In the process of catalytic oxidation of NO, semiconductor catalysts absorb the energy of photons to generate separated photogenerated carriers. Electrons and holes combine with oxygen and water to produce superoxide radicals and hydroxyl radicals, etc., which are highly oxidizing free radical species, so that NO is oxidized into non-toxic nitrogen-containing species. However, the commonly used photocatalyst materials currently have problems such as easy recombination of carriers, poor visible light absorption, and easy generation of toxic byproducts, which affect the final catalytic effect. Therefore, it is necessary to develop a new and efficient photocatalyst to solve the problems of carrier dynamics and thermodynamics to improve the NO removal rate.
[0003] Perylene compounds are a class of aromatic compounds composed of five fused benzene rings. Their structure is easy to modify. Various functional groups can be introduced by utilizing the chemically active sites at the bay position of the perylene ring and by utilizing the anhydride and amide derivatives of perylene. They have been widely developed in the fields of material science, biology, and medicine, and have great application potential. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a preparation method and application of a perylene metal compound and a composite material thereof.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] One of the technical solutions of the present invention is to provide a method for preparing a perylene metal compound, comprising the following steps:
[0007] The perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) is reacted with a metal organic compound to prepare a perylene metal compound.
[0008] Furthermore, the metal in the metal organic compound is selected from any one of Ti, Zr, Co or Ce.
[0009] Preferably, the metal organic compound is tetrabutyl titanate.
[0010] Furthermore, the molar ratio of the perylene-3,4,9,10-tetracarboxylic dianhydride to the metal ion in the metal organic compound is 1:2.
[0011] Preferably, the amount of the metal organic compound added is 105 μL, 205 μL, or 305 μL.
[0012] Further, perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) and the metal organic compound are ultrasonically mixed in a NaOH aqueous solution to form a suspension, and then a subsequent reaction is performed.
[0013] The preferred concentration of the NaOH aqueous solution is 1.4 mol / L.
[0014] Furthermore, the reaction method for the suspension to react is a microwave method, a hydrothermal method or an oil bath method, and the corresponding reactors are a polytetrafluoroethylene microwave reactor, a hydrothermal reactor or a flask lined with polytetrafluoroethylene.
[0015] Furthermore, the reaction temperature is 90-180° C., and the reaction time is 30 min-24 h. When the microwave reaction temperature is lower than 90° C. or higher than 180° C., and the reaction time is lower than 30 min, the final perylene metal compound cannot be formed.
[0016] Preferably, the microwave reaction temperature is selected from 90°C, 120°C, 150°C or 180°C, and the microwave reaction time is selected from 30 min, 60 min or 90 min.
[0017] More preferably, the microwave reaction temperature is 150° C. and the microwave reaction time is 30 min.
[0018] Furthermore, the prepared perylene metal compound has a flower ball-like structure.
[0019] The second technical solution of the present invention is to provide a method for preparing a perylene-based metal compound composite material, comprising the following steps:
[0020] The perylene-3,4,9,10-tetracarboxylic dianhydride, a metal organic compound and a two-dimensional nanomaterial are reacted to prepare a perylene-based metal compound.
[0021] Furthermore, the metal in the metal organic compound is selected from any one of Ti, Zr, Co or Ce.
[0022] Preferably, the metal organic compound is tetrabutyl titanate.
[0023] Furthermore, the two micro-nano materials are selected from any one of GO, Mexene, and MoS2.
[0024] Preferably, the two-dimensional nanomaterial is GO.
[0025] Furthermore, the molar ratio of the perylene-3,4,9,10-tetracarboxylic dianhydride to the metal ion in the metal organic compound is 1:2, and the mass ratio of the perylene-3,4,9,10-tetracarboxylic dianhydride to the two-dimensional nanomaterial is 5:1.
[0026] Preferably, the amount of the metal organic compound added is 105 μL, 205 μL, or 305 μL.
[0027] Further, perylene-3,4,9,10-tetracarboxylic dianhydride, the metal organic compound and the two-dimensional nanomaterial are ultrasonically mixed in a NaOH aqueous solution to form a suspension for subsequent reaction.
[0028] The preferred concentration of the NaOH aqueous solution is 1.4 mol / L.
[0029] Furthermore, the reaction method for the suspension to react is a microwave method, a hydrothermal method or an oil bath method, and the corresponding reactors are a polytetrafluoroethylene microwave reactor, a hydrothermal reactor or a flask lined with polytetrafluoroethylene.
[0030] Furthermore, the reaction temperature is 90-180° C., and the reaction time is 30 min-24 h. When the microwave reaction temperature is lower than 90° C. or higher than 180° C., and the reaction time is lower than 30 min, the final perylene metal compound composite material cannot be formed.
[0031] Preferably, the microwave reaction temperature is selected from 90°C, 120°C, 150°C or 180°C, and the microwave reaction time is selected from 30 min, 60 min or 90 min.
[0032] More preferably, the microwave reaction temperature is 150° C. and the microwave reaction time is 30 min.
[0033] Furthermore, the perylene-based metal compound in the prepared perylene-based metal compound composite material presents a two-dimensional layered structure on the two-dimensional nanostructure.
[0034] The third technical solution of the present invention is to provide an application of a perylene metal compound and a composite material thereof, wherein the perylene metal compound and the composite material thereof are used as a photocatalyst for the photocatalytic oxidation reaction of NO.
[0035] During the entire photocatalytic oxidation of NO reaction, perylene-based metal compounds and their composites have certain structural stability and photocatalytic activity.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The present invention adopts microwave synthesis technology to avoid the collapse of the pore structure of the perylene metal compound and its composite material, and at the same time facilitates the rapid nucleation and crystallization of crystals. The porous structure of the perylene metal compound and its composite material in the present invention increases the number of catalytic active sites in the reaction, is conducive to the gas phase adsorption of NO, and increases the conversion rate of NO oxidation.
[0038] (2) The absorption band edge of the PTCDA ligand molecule in the perylene metal compound and the composite material prepared by the present invention is about 620nm, and its band gap Eg can be calculated to be about 1.95eV through Kubelka-Munk transformation, while the visible light absorption band edge of the prepared Ti-PTCDA is around 550nm, and its band gap is calculated to be about 2.25eV, so the visible light absorption is enhanced and the NO oxidation performance is improved. The enrichment of holes in the valence band can directly oxidize NO to NO3 - , which is selective for the oxidation of NO and avoids the formation of toxic byproducts of NO2.
[0039] (3) The perylene metal compounds and composite materials prepared by the present invention realize the spatial separation of photogenerated carriers through the good conductivity of the two-dimensional nanomaterials, and the superhot spots generated by the interaction between the selected two-dimensional nanomaterials and the microwave field promote the in-situ nucleation and crystallization of the perylene metal compounds.
[0040] (4) The perylene metal compound and the composite material thereof prepared by the present invention are used as photocatalysts, and the preparation method is simple, the conditions are mild and clean, and basically no environmental pollution is generated during the preparation process.
[0041] (5) The chemical reagents used in the present invention are all commonly used reagents, cheap and easily available. Compared with other traditional methods for synthesizing materials, this method has the advantages of low energy consumption, rapid controllability and precise coordination synthesis. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1Transmission electron microscope images of the perylene metal compound prepared in Example 11 of the present invention and the perylene metal compound composite material prepared in Example 5: a and c are transmission electron microscope images of the flower ball structure of Ti-PTCDA samples of different scales, wherein the scale of Figure a is 200nm, and the scale of c is 20nm. In addition, the selected area electron diffraction image of the Ti-PTCDA sample is in the upper right corner of Figure c; b is a high-resolution transmission electron microscope image of the Ti-PTCDA / rGO sample, with a scale of 10nm; d is a high-resolution transmission electron microscope image of the Ti-PTCDA sample, with a scale of 5nm; eh is an element mapping image of Ti-PTCDA, wherein e is a total element map, f is C element, g is O element, and h is Ti element. Among them, Ti-PTCDA is the prepared perylene metal compound, and Ti-PTCDA / rGO is the prepared perylene metal compound composite material.
[0043] Figure 2 The XRD patterns of the perylene metal compound prepared in Example 11 of the present invention and the perylene metal compound composite material prepared in Example 5, wherein Ti-PTCDA is the prepared perylene metal compound, and Ti-PTCDA / rGO is the prepared perylene metal compound composite material.
[0044] Figure 3 The NO oxidation performance under a xenon lamp of the perylene metal compound prepared in Example 11 of the present invention and the perylene metal compound composite material prepared in Example 5 is compared. Ti-PTCDA is the prepared perylene metal compound, and Ti-PTCDA / rGO is the prepared perylene metal compound composite material. DETAILED DESCRIPTION
[0045] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0046] In the following examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.
[0047] Embodiment 1:
[0048] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a 100 mL flask and heated in an oil bath at 150 ° C, reacted for 24 hours, and cooled to room temperature. The solid product was washed with deionized water by centrifugation and dried at 80 ° C to form a light yellow powder. By comparison Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0049] Embodiment 2:
[0050] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a 60 mL polytetrafluoroethylene-lined hydrothermal reactor, the temperature in the hydrothermal reactor was programmed to 150 ° C and kept warm for 24 hours, and then cooled to room temperature. The solid product was centrifuged and washed with deionized water, dried at 80 ° C to form a yellow powder, and compared. Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0051] Embodiment 3:
[0052] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a polytetrafluoroethylene microwave reactor and heated to 90°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 90°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water to remove the solid product. It was dried at 80°C to form an orange powder, which was compared with Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0053] Embodiment 4:
[0054] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 120°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 120°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was compared with Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0055] Embodiment 5:
[0056] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was then Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0057] Embodiment 6:
[0058] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a polytetrafluoroethylene microwave reactor and heated to 180°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 180°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was compared with Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0059] Embodiment 7:
[0060] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 60 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was compared with Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0061] Embodiment 8:
[0062] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 90 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was compared with Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0063] Embodiment 9:
[0064] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 205 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was compared with Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0065] Embodiment 10:
[0066] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 305 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was compared with Figure 2 The XRD pattern shows that the powder is a composite material of perylene-based metal compounds.
[0067] Embodiment 11:
[0068] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form an orange powder, which was then Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0069] Embodiment 12:
[0070] Add 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) to 50 mL of NaOH aqueous solution (1.4 mol / L) and stir to form a transparent brown solution. Add 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) to the brown solution. After that, stir and ultrasonicate the mixture for 30 minutes to form a suspension. Transfer the suspension to a 100 mL flask and heat it in an oil bath at 150°C, react for 24 hours, and cool to room temperature. Wash the solid product with deionized water by centrifugation, dry it at 80°C to form a powder, and compare the XRD images of the samples. Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0071] Embodiment 13:
[0072] Add 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) to 50 mL of NaOH aqueous solution (1.4 mol / L) and stir to form a transparent brown solution. Add 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) to the brown solution. Then, stir and ultrasonicate the mixture for 30 minutes to form a suspension. Transfer the suspension to a 60 mL polytetrafluoroethylene-lined hydrothermal reactor, raise the temperature to 150°C in the hydrothermal reactor for 24 hours, and cool to room temperature. Centrifuge and wash the solid product with deionized water, dry at 80°C to form a powder, and compare the XRD images of the samples. Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0073] Embodiment 14:
[0074] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a polytetrafluoroethylene microwave reactor and heated to 90°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 90°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water to remove the solid product. Dry at 80°C to form a powder, and compare the XRD image of the sample with Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0075] Embodiment 15:
[0076] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 120°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 120°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. It was dried at 80°C to form a powder, and the XRD pattern of the sample was compared with Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0077] Embodiment 16:
[0078] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a polytetrafluoroethylene microwave reactor and heated to 180°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 180°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. Dry at 80°C to form a powder, and the XRD pattern of the sample was compared with Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0079] Embodiment 17:
[0080] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 60 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. Dry at 80°C to form a powder, and the XRD pattern of the sample was compared with Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0081] Embodiment 18:
[0082] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 90 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. Dry at 80°C to form a powder, and the XRD pattern of the sample was compared with Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0083] Embodiment 19:
[0084] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 205 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. Dry at 80°C to form a powder, and the XRD pattern of the sample was compared with Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0085] Embodiment 20:
[0086] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 305 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the brown solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The mixture was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. Dry at 80°C to form a powder, and the XRD pattern of the sample was compared with Figure 2 The XRD pattern shows that the powder is a perylene metal compound.
[0087] Comparative Example 1:
[0088] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of NaOH aqueous solution (1.4 mol / L) and stirred to form a transparent brown solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) and 24 mg of GO powder were added to the brown solution. The mixture was then stirred and ultrasonicated for 30 min and the solid product was centrifuged and washed with deionized water. It was dried at 80 °C to form a powder.
[0089] Comparative Example 2:
[0090] 118 mg of perylene-3,4,9,10-tetracarboxylic dianhydride (PTCDA) was added to 50 mL of aqueous solution and stirred to form a transparent solution. 105 μL of tetrabutyl titanate (Ti:PTCDA (mol / mol) = 2:1) was added to the solution. After that, the mixture was stirred and ultrasonicated for 30 minutes to form a suspension. The suspension was transferred to a polytetrafluoroethylene microwave reactor and heated to 150°C within 15 minutes by a programmed microwave digestion system. After the microwave reactor was kept at 150°C for 30 minutes, it was cooled to room temperature. The solid product was centrifuged and washed with deionized water. Dry at 80°C to form a powder.
[0091] The samples of the perylene metal compounds and the composite materials thereof prepared in the above examples and comparative examples were structurally characterized by the following method:
[0092] (1) X-ray diffraction (XRD, Bruker D8 ADVANCE) was used to characterize the crystal structure of the samples;
[0093] (2) Transmission electron microscopy (SEM, FEI Quanta FEG) was used to characterize the micromorphology and structure of the samples.
[0094] The method for testing the performance of the samples of the perylene metal compounds and the composite materials thereof prepared in the above embodiments and comparative examples in the photocatalytic process comprises the following steps:
[0095] (1) In a continuous flow reactor, the reactor surface is sealed with quartz glass;
[0096] (2) In each experiment, simulated exhaust gas containing 500 ppb NO was passed through a reactor containing 0.10 g of sample at a rate of 2.0 L / min.
[0097] (3) After 30 min of dark adsorption, when the photocatalyst is in an adsorption-desorption equilibrium state, a 300 W xenon lamp is turned on to simulate sunlight for photocatalytic reaction.
[0098] (4) Using NO-NO2-NO X A dynamic analyzer (Thermo Scientific 42i-TL) was used to monitor the concentration changes of NO and NO2 online.
[0099] like Figure 1As shown, the transmission electron microscope (TEM), high-resolution transmission electron microscope (HRTEM), selected area electron diffraction images and corresponding element mapping diagrams of the perylene metal compound prepared in Example 11 and the perylene metal compound composite material prepared in Example 5. From a, it can be seen that the perylene metal compound Ti-PTCDA synthesized by microwave method has a flower ball structure. In b, Ti-PTCDA in the composite sample Ti-PTCDA / rGO is evenly distributed on rGO to form a two-dimensional layered structure. The (110) plane and the (002) plane correspond to the lattice spacing of 0.67nm for the Ti-PTCDA lattice fringes in Ti-PTCDA / rGO and the lattice spacing of 0.34nm for the rGO lattice fringes, respectively. It can also be seen from the figure that Ti-PTCDA and rGO are successfully composited. From c and d, it can be seen that the clear Ti-PTCDA lattice fringes correspond to lattice spacings of 0.67nm, 0.40nm and 0.36nm. The inserted selected area electron diffraction image shows the polycrystalline rings of the sample, corresponding to the (110), (201) and (001) planes of the X-ray diffraction of Ti-PTCDA.
[0100] like Figure 2 As shown, the XRD spectra of the perylene metal compound prepared in Example 11 and the perylene metal compound composite material prepared in Example 5; wherein the horizontal axis is the angle and the vertical axis is the intensity. It can be seen from the XRD spectrum that the Ti-PTCDA synthesized in situ by microwave method has a higher degree of crystallinity, and Ti-PTCDA / rGO is successfully composited together.
[0101] like Figure 3 As shown, the NO oxidation performance of the perylene metal compound prepared in Example 11 and the perylene metal compound composite material prepared in Example 5 under the irradiation of a xenon lamp; the figure further confirms that the perylene metal compound and its composite material have high conversion rate and high selectivity for NO oxidation.
[0102] The perylene metal compounds and their composite materials synthesized in situ by microwave were placed in a continuous flow reactor and photocatalytic reactions were carried out using a 300W xenon lamp to simulate sunlight. X The dynamic analyzer (Thermo Scientific 42i-TL) continuously measured the changes in NO and NO2 concentrations. The performance tests were performed on the embodiments and comparative examples, and the results are shown in Table 1:
[0103] Table 1 Photocatalytic performance of perylene metal compounds and their composites
[0104]
[0105] It can be seen that the perylene metal compound and its composite material prepared by the method of the present invention have better performance, higher NO removal rate and lower NO2 selectivity (1.5%), while in Comparative Example 1, due to the mechanical mixing of Ti-PTCDA and rGO, the two failed to composite, so the performance was lower than that of the microwave-prepared sample. In Comparative Example 2, when the pure solvent was water, the sample synthesis rate was low and there were more impurities, thus showing a poor NO removal effect.
[0106] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a perylene metal compound, characterized in that: The following steps are involved: Perylene-3,4,9,10-tetracarboxylic dianhydride and a metal organic compound are ultrasonically mixed in a 1.4 mol / L NaOH aqueous solution to form a suspension, and subjected to microwave reaction to prepare a perylene metal compound; Wherein, the molar ratio of the perylene-3,4,9,10-tetracarboxylic dianhydride to the metal ion in the metal organic compound is 1:2; The metal organic compound is tetrabutyl titanate; During the microwave reaction, the reaction temperature was 150°C and the reaction time was 30 min.
2. A perylene metal compound, characterized in that: Prepared by the preparation method of claim 1, the perylene metal compound has a flower ball-like structure.
3. A method for preparing a perylene-based metal compound composite material, characterized in that: The following steps are involved: Perylene-3,4,9,10-tetracarboxylic dianhydride, metal organic compound and two-dimensional nanomaterial are ultrasonically mixed in 1.4 mol / L NaOH aqueous solution to form a suspension, and microwave reaction is performed to prepare a perylene metal compound composite material; The molar ratio of the perylene-3,4,9,10-tetracarboxylic dianhydride to the metal ion in the metal organic compound is 1:2, and the mass ratio of the perylene-3,4,9,10-tetracarboxylic dianhydride to the two-dimensional nanomaterial is 5:
1. The metal organic compound is tetrabutyl titanate, and the two-dimensional nanomaterial is GO; During the microwave reaction, the reaction temperature was 150°C and the reaction time was 30 min.
4. A perylene-based metal compound composite material, characterized in that: Prepared by the preparation method of claim 3, the perylene-based metal compound in the perylene-based metal compound composite material presents a two-dimensional layered structure on a two-dimensional nanostructure.
5. Use of the perylene metal compound according to claim 2 or the perylene metal compound composite material according to claim 4, characterized in that: The perylene metal compound and the composite material thereof are used as a photocatalyst for photocatalytic oxidation reaction of NO.
Citation Information
Patent Citations
Preparation method for simultaneously obtaining porous metal oxide nano material and high-purity perylene
CN102795603A
Preparation and photocatalytic hydrogen generation performance of N-pyridyl perylenetetracarboxylic diimide
CN104557931A
Preparation method and application of perylene bisimide based organometallic polymer with visible-light photocatalytic performance
CN105749978A
Preparation method and application of polymer dots containing perylene bisimide
CN105924642A
Polyaniline / perylene bisimide organic heterojunction photocatalyst and preparation method and application thereof
CN111495426A