A method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by using segmented treatment

Through segmented treatment and catalytic oxidation technology, combined with the use of lime mortar and ultrafiltration membrane components, the problems of high cost of tin and lead ore ore treatment wastewater and low removal efficiency are solved, and efficient wastewater reuse and efficiency improvement of ore production are achieved. .

CN115636537BActive Publication Date: 2024-11-08GUANGXI GAOFENG MINE IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211338938.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-11-08
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

The prior art is costly and difficult to effectively remove heavy metals and organic matters when treating tin lead ore ore wastewater, affects the environment and production efficiency, and fails to make full use of wastewater resources.

Method used

The segmented treatment method is adopted, including collecting ore-dressing wastewater for pre-precipitation and pH adjustment, using catalytic oxidation and lime mortar for precipitation, and then further treatment through the ultrafiltration membrane assembly to ensure that the quality of the wastewater meets the reuse standards.

Benefits of technology

It reduces the cost of wastewater treatment, improves resource utilization, realizes effective recycling of wastewater, improves the water quality and product recovery rate of ore dressing production, simplifies the operating process, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003915672360000051
    Figure BDA0003915672360000051
  • Figure BDA0003915672360000052
    Figure BDA0003915672360000052
Patent Text Reader

Abstract

A method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment, comprising collecting the dressing wastewater and pre-precipitating it, introducing sulfuric acid to adjust the pH of the wastewater and then precipitating it, returning part of the wastewater to the sanitary water of the dressing plant process site; treating the remaining wastewater by catalytic oxidation, adjusting the pH by lime slurry and precipitating it, returning part of the dressing wastewater to the grinding sand pump jigging operation water after precipitation; and treating the remaining wastewater by ultrafiltration membrane assembly after precipitation, and then reuse it in the flotation process. The present invention can be used according to the water quality requirements of each operation point of the ore dressing plant, and after targeted and appropriate treatment, it can be returned to each operation point of the ore dressing after the treatment is completed, so as to achieve the goal of improving the resource utilization rate of the ore dressing plant wastewater and improve the recovery rate of minerals such as lead and zinc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater resource utilization, and in particular to a method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by adopting segmented treatment. Background Art

[0002] Tin-lead ore is usually an associated ore with complex mineral properties. Oxide ores and sulfide ores coexist closely. Its associated minerals include various valuable substances such as lead, zinc, antimony, arsenic, sulfur, and iron. Therefore, tin ore dressing is relatively complicated. Its beneficiation process is generally: magnetic separation-flotation-gravity separation. A large amount of beneficiation wastewater is generated during the beneficiation process. The beneficiation wastewater at each operation point has complex properties. The volume of this part of wastewater is large and the content of heavy metals is high. Due to the addition of many flotation agents such as yellow medicine, black medicine, sodium cyanide and other substances, the beneficiation wastewater contains a large amount of organic matter. It is difficult to manage and the cost is high. Conventional beneficiation plants return the wastewater to the beneficiation plant for use after unified management, so the cost is high and the beneficiation indicators are unsatisfactory. If a large amount of beneficiation wastewater is not treated and directly discharged into the environment, it will cause serious environmental pollution. The beneficiation process requires the use of a large amount of fresh make-up water. If the beneficiation wastewater can be comprehensively treated and reused in beneficiation production, it can not only save a lot of fresh water resources, but also avoid environmental pollution.

[0003] Chinese patent CN104071939B discloses a method for the coordinated treatment of non-ferrous metal mine wastewater and mining mine water, wherein oxidants such as ozone and hydrogen peroxide are introduced under stirring and ultraviolet irradiation conditions for deep oxidation treatment, and Fe 2+ The reagent is catalytically oxidized. Although the pH is adjusted to perform coagulation and precipitation reactions, this method uses a variety of oxidation technologies to treat wastewater. Its deep oxidation produces a large number of hydroxyl radicals in the water body, which can decomplex the organic-heavy metal complex in the wastewater, thereby achieving the effect of removing heavy metals and organic matter in the coagulation and precipitation process. However, this method ignores the reaction rate of ultraviolet light and ozone. Ozone and ultraviolet light are both slow chemical reaction processes. If they react synergistically with the Fenton reaction, the operating cost will be greatly increased, and it is difficult to be widely used in industrial applications.

[0004] Chinese patent CN106242191B discloses a treatment process for lead-zinc ore beneficiation wastewater, which uses calcium hydroxide for pretreatment to adjust the pH of the beneficiation wastewater to 7-8, and then the completely precipitated supernatant is passed into the ozone tank for the first stage of oxidation treatment, and the treated wastewater is passed into the A / O process for biochemical treatment. Although it is then transferred to the second stage of ozone treatment, this method uses a pre-precipitation process to effectively reduce the impact of heavy metals and SS on subsequent processes. At the same time, the introduction of ozone for pretreatment can enhance the removal effect of the A / O process on organic matter, and finally the use of ozone secondary oxidation greatly guarantees the removal effect of the wastewater. Similar to the above example, this method fails to fully consider the application scenarios of the ozone process. At the same time, if the removal effect of heavy metals is not guaranteed in the pretreatment process, it will greatly affect the removal efficiency of organic matter in the beneficiation wastewater. At the same time, due to the low biodegradability of the beneficiation wastewater, it is worth discussing the use of biochemical processes for treatment. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment. The treated dressing wastewater is recycled and reused in the ore dressing production process without affecting the product recovery rate and product grade. The process is stable and easy to operate.

[0006] To achieve the above-mentioned purpose, the technical scheme of the present invention is to provide a method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment, including collecting the dressing wastewater and pre-precipitating it, introducing sulfuric acid to adjust the pH of the wastewater and then precipitating it, returning part of the wastewater to the sanitary water of the dressing plant process site; treating the remaining wastewater by catalytic oxidation, adjusting the pH by lime slurry and precipitating it, and returning part of the dressing wastewater after precipitation to the grinding sand pump jigging operation water; the remaining wastewater is precipitated and treated by an ultrafiltration membrane assembly, and then returned to the flotation process. The specific operation steps are as follows:

[0007] (1) adding sulfuric acid solution to the mineral processing wastewater, stirring at a stirring speed of 50-100 r / min for 10-20 min, collecting the mixed solution A after the stirring is completed, and recycling 5% of the mixed solution A to the site cleaning pool;

[0008] (2) Add ferrous sulfate to the mixed solution A, stir at a speed of 50-100 r / min for 10-20 min, then add 30% hydrogen peroxide, stir at 50-100 r / min for 45-90 min, and collect the mixed solution B after the stirring is completed;

[0009] (3) adding lime liquid to the mixed liquid B, stirring at a stirring speed of 50-100 r / min for 60-120 min, standing for 30-60 min, collecting the supernatant C, and recycling 30% of the supernatant C to the grinding and jigging production process;

[0010] (4) The remaining supernatant C is passed into a polytetrachloroethylene ultrafiltration membrane assembly and pumped at a suction pressure of 0.50 MPa-3.0 MPa. After being treated by the membrane system, the wastewater is reused in the flotation and shaking table production processes.

[0011] In step (2), the ferrous sulfate is added to the mixed solution A in a weight ratio of mixed solution A: ferrous sulfate = 10000: 3.6, and the hydrogen peroxide is added in a ratio of mixed solution A: oxidant = 10000: 15.

[0012] In step (3), the lime slurry is added to the mixed solution B in a weight ratio of mixed solution B: lime slurry = 10000: 2.8.

[0013] The membrane assembly described in step (4) is an ultrafiltration membrane made of polytetrafluoroethylene.

[0014] The concentration of sulfuric acid in step (1) is 10%.

[0015] The order of adding the catalyst ferrous sulfate and the oxidant hydrogen peroxide in step (2) cannot be changed. The catalyst ferrous sulfate should be added first and then the oxidant hydrogen peroxide, so that the hydrogen peroxide will not be consumed first by the ferrous ions in the wastewater, resulting in the loss of the strong oxidizing hydroxyl radicals generated by its hydrolysis, thereby affecting the treatment effect of the mineral processing wastewater.

[0016] Furthermore, the method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment comprises the following steps:

[0017] (1) Add sulfuric acid solution to the mineral processing wastewater, stir at a stirring speed of 50-100 r / min for 10-20 min, and collect the mixed solution A after the stirring is completed.

[0018] (2) Add ferrous sulfate to mixed solution A, stir at a speed of 50-100 r / min for 10-20 min, then add hydrogen peroxide (30%), stir at 50-100 r / min for 45-90 min, and collect mixed solution B after stirring.

[0019] (3) Add lime solution to the mixed solution B, stir for 60-120 min at a stirring speed of 50-100 r / min, let stand for 30-60 min, and collect the supernatant C;

[0020] (4) The supernatant C is passed into a polytetrachloroethylene ultrafiltration membrane assembly and pumped at a suction pressure of 0.50 MPa-3.0 MPa. After being treated by the membrane system, wastewater meeting the reuse standard is obtained.

[0021] The beneficial effects of the present invention are:

[0022] 1. According to the different water quality requirements of each production process of the mineral processing technology, the appropriate segmented treatment is adopted to accurately control the amount of recycled water and the recycling link, which effectively reduces the cost of wastewater treatment, improves resource utilization, and achieves the purpose of wastewater reuse.

[0023] 2. In view of the characteristics of tin-lead polymetallic ore beneficiation wastewater, catalytic oxidation is used for treatment, which can break down the metal complexes in the beneficiation wastewater and turn the metal ions in the beneficiation wastewater into ionic state. At the same time, it can also break down the organic matter in the wastewater, greatly reducing the difficulty of removing COD in the wastewater.

[0024] 3. As lime slurry has a strong coagulation and sedimentation effect, lime slurry is used to adjust pH. In this process, no other organic polymer flocculants need to be added, which is conducive to the reuse of wastewater in the mineral processing system after the wastewater reaches the standard. If the alkali solution selected for adjustment is used, polyacrylamide and other flocculants need to be used for coagulation and sedimentation, and a large amount of polyacrylamide will affect the reuse of mineral processing wastewater and the recovery rate of tin polymetallic ore.

[0025] 4. Lime precipitation has been used in the early stage to improve the effect of coagulation and precipitation, increase the precipitation time, and enhance its precipitation effect. Therefore, the last process uses ultrafiltration membrane components to avoid membrane pollution and concentration polarization, effectively ensuring the treatment effect of mineral processing wastewater. The ultrafiltration membrane is selected as the last guarantee process, with a small transmembrane pressure and a wear-resistant material, which can ensure the treatment efficiency of mineral processing wastewater.

[0026] 5. The operation process is simple and convenient for industrial application. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further described in detail below through specific embodiments.

[0028] Example 1

[0029] This embodiment is a specific example of the method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment according to the present invention, comprising the following steps:

[0030] The ore dressing wastewater produced by a ore dressing plant in Dachang mining area, Nandan County, Hechi City, Guangxi was selected. The ore dressing wastewater was the wastewater generated in the tin polymetallic ore dressing process, with a pH of 12.23, Cu of 0.04 mg / L, Pb of 1.06 mg / L, Zn of 1.84 mg / L, As of 0.022 mg / L, and Sb of 5.800 mg / L. The pH value of the mineral processing wastewater was adjusted to 3 using 10% sulfuric acid solution, and 5% of the treated wastewater was pumped back to the ground cleaning pool. The remaining wastewater was stirred for 10 minutes at a stirring speed of 50r / min, and then ferrous sulfate was added at a stirring speed of 50r / min for 10 minutes, and then hydrogen peroxide was added and stirred for 45 minutes at a stirring speed of 50r / min. After the stirring was completed, the mixed solution was collected, and lime solution was added to the mixed solution, and stirred for 60 minutes at a stirring speed of 50r / min. After standing for 30 minutes, a supernatant was obtained, and 30% of the supernatant was reused in the grinding and jigging processes. Subsequently, the remaining supernatant was passed into a polytetrachloroethylene ultrafiltration membrane assembly and pumped at a suction pressure of 1.50MPa. After being treated by the membrane system, experimental water sample 1 was obtained.

[0031] Example 2

[0032] This embodiment is another specific example of the method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment according to the present invention, comprising the following steps:

[0033] The same mineral processing wastewater sample in Example 1 was used, and the pH value of the mineral processing wastewater was adjusted to 2 using a 10% sulfuric acid solution. 5% of the treated wastewater was pumped back to the ground cleaning pool, and the remaining wastewater was stirred for 15 minutes at a stirring speed of 75 r / min. Then ferrous sulfate was added and stirred for 15 minutes at a stirring speed of 75 r / min. Then hydrogen peroxide was added and stirred for 70 minutes at a stirring speed of 75 r / min. After the stirring was completed, the mixed solution was collected, lime solution was added to the mixed solution, and stirred for 90 minutes at a stirring speed of 75 r / min. The mixture was allowed to stand for 45 minutes to obtain a supernatant, and 30% of the supernatant was reused in the grinding and jigging processes. The supernatant was then passed into a polytetrachloroethylene ultrafiltration membrane assembly and pumped at a suction pressure of 2.0 MPa. After being treated by the membrane system, experimental water sample 2 was obtained.

[0034] Example 3

[0035] This embodiment is another specific example of the method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment according to the present invention, comprising the following steps:

[0036] The same mineral processing wastewater sample in Example 1 was used, and the pH value of the mineral processing wastewater was adjusted to 3.5 using a 10% sulfuric acid solution. 5% of the treated wastewater was pumped back to the ground cleaning pool, and the remaining wastewater was stirred for 20 minutes at a stirring speed of 100 r / min. Then ferrous sulfate was added and stirred for 20 minutes at a stirring speed of 100 r / min. Then hydrogen peroxide was added and stirred for 90 minutes at a stirring speed of 100 r / min. After the stirring was completed, the mixed solution was collected, lime solution was added to the mixed solution, and stirred for 120 minutes at a stirring speed of 100 r / min. The mixture was allowed to stand for 60 minutes to obtain a supernatant. 30% of the supernatant was reused in the grinding and jigging processes. The supernatant was then passed into a polytetrachloroethylene ultrafiltration membrane assembly and pumped at a suction pressure of 3.0 MPa. After being treated by the membrane system, experimental water sample 3 was obtained.

[0037] The experimental water samples 1-3 were subjected to open-circuit beneficiation tests, mainly to investigate the effect of water samples on the concentrate grade and Pb metal recovery rate of lead flotation from magnetic tailings of tin polymetallic ores, as well as the loss rate of zinc in lead concentrate. The magnetic tailings were taken once every 30 minutes, and the sampling period was 8 hours. The fine mud was first separated from the taken ore samples and stirred evenly, and then divided into each ore sample. The open-circuit beneficiation condition test was conducted to conduct flotation lead concentrate tests, and the lead-zinc concentrate and tailings were dehydrated, dried, weighed, reduced, sampled, and the Pb and Zn grades in the concentrate and tailings were analyzed. The recovery rates are shown in Table 2.

[0038] The experimental water samples obtained from implementation cases 1-3 were tested, and the heavy metal removal efficiency basically reached the Class III standard in Table 1 of the "Surface Water Environment" (GB38-2002), but the COD removal effect did not meet the Class III surface water standard, but had reached the Level A standard in the "Integrated Emission Standard for Urban Sewage Treatment Plants".

[0039] Table 1 Water quality test results

[0040]

[0041] Table 2 Experimental water sample recovery test results

[0042]

[0043] The mineral processing experiments show that the treated mineral processing wastewater provided by the present invention is used in the mineral processing experiments, and the flotation product recovery rate and grade are increased by 2-5%. This shows that the mineral processing wastewater treated by the method described in the present invention can meet the water demand in the mineral processing process, and the moderate treatment method effectively reduces the wastewater treatment cost and reduces the water cost in mineral processing production.

[0044] The above content is a detailed explanation of the present invention in combination with specific implementation methods. Those skilled in the art should understand that the specific implementation methods of the present invention are not limited to this explanation. Without departing from the concept of the present invention, corresponding optimizations and improvements can be made, which should be regarded as the protection scope of the present invention.

Claims

1. A method for improving the resource utilization rate of tin-lead polymetallic ore dressing wastewater by staged treatment, comprising collecting the dressing wastewater and pre-precipitating it, introducing sulfuric acid to adjust the pH of the wastewater and then precipitating it, returning part of the wastewater to the sanitary water of the dressing plant process site; treating the remaining wastewater by catalytic oxidation, adjusting the pH by lime slurry and precipitating it, returning part of the dressing wastewater after precipitation to the grinding sand pump jigging operation water; the remaining wastewater is precipitated and treated by an ultrafiltration membrane module and then returned to the flotation process, and the specific operation steps are as follows: (1) Add sulfuric acid solution to the mineral processing wastewater, stir at a stirring speed of 50-100r / min for 10-20min, collect the mixed solution A after stirring, and reuse 5% of the mixed solution A in the site cleaning pool; (2) Add ferrous sulfate to the mixed solution A, stirring at a speed of 50-100 r / min for 10-20 min, then add hydrogen peroxide, stirring at 50-100 r / min for 45-90 min, and collect the mixed solution B after the stirring is completed; In step (2), the ferrous sulfate is added to the mixed solution A in a weight ratio of mixed solution A: ferrous sulfate = 10000: 3.6, and the hydrogen peroxide is added in a ratio of mixed solution A: oxidant = 10000: 15; (3) Add lime slurry to the mixed liquid B, stir for 60-120 min at a stirring speed of 50-100 r / min, let stand for 30-60 min, collect the supernatant C, and reuse 30% of the supernatant C in the grinding and jigging production process; (4) The remaining supernatant C is passed into a polytetrachloroethylene ultrafiltration membrane assembly and pumped at a suction pressure of 0.50 MPa-3.0 MPa. After being treated by the membrane system, the wastewater is reused in the flotation and shaking table production processes.

2. The method for improving resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment according to claim 1 is characterized in that: The concentration of the sulfuric acid solution in step (1) is 10%.

3. The method for improving resource utilization rate of tin-lead polymetallic ore dressing wastewater by segmented treatment according to claim 1 is characterized in that: In step (3), the lime slurry is added to the mixed solution B in a weight ratio of mixed solution B: lime slurry = 10000:2.8.