Integrated molecular beam epitaxial crucible manufacturing method, epitaxial crucible and molecular beam source furnace
By embedding the heating wire into the pyrolyzed boron nitride layer, the problems of low heating efficiency and difficult installation of the molecular beam source furnace are solved, and efficient and low-cost molecular beam epitaxial crucible and source furnace design are achieved.
Patent Information
- Application Number
- CN202211378289.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-04
AI Technical Summary
The existing molecular beam source furnaces have low peripheral heating efficiency and difficult installation, resulting in high cost and low efficiency, and lack of effective solutions.
The integrated molecular beam epitaxial crucible production method is adopted to embed the heating wire into the pyrolytic boron nitride layer, and the heating wire is fixed through the preparation process of the pyrolytic boron nitride layer divided into two stages, simplifying the production process and improving thermal efficiency.
It realizes a molecular beam epitaxial crucible and source furnace with simple structure, low cost, high efficiency, uniform thermal field and outstanding thermal insulation effect, reducing production costs and improving thermal efficiency.
Smart Images

Figure CN115637490B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of epitaxial growth, and in particular to a method for manufacturing an integrated molecular beam epitaxial crucible, an epitaxial crucible and a molecular beam source furnace. Background Art
[0002] Molecular beam epitaxial growth technology is an advanced technology for growing semiconductor thin film materials in an ultra-high vacuum environment.
[0003] During molecular beam epitaxial growth, the molecular beam source furnace is powered on to heat the solid or liquid material stored in its crucible, causing the material to evaporate and then be sprayed along the crucible mouth into the substrate sheet in the vacuum chamber to be deposited to form a thin film material.
[0004] Existing molecular beam source furnaces generally use heating wires installed in the air around the crucible to heat the crucible. The thermal efficiency is low and the heating wires need to be adjusted and fixed by mounting components such as support rings, which makes installation difficult, resulting in high production costs and low production efficiency of molecular beam source furnaces.
[0005] There is currently no effective technical solution to the above problems. Summary of the invention
[0006] The purpose of the present application is to provide an integrated molecular beam epitaxial crucible manufacturing method, an epitaxial crucible and a molecular beam source furnace, so as to improve the thermal efficiency of the molecular beam source furnace, reduce the manufacturing cost and improve the manufacturing efficiency.
[0007] In a first aspect, the present application provides a method for manufacturing an integrated molecular beam epitaxy crucible, which is used to manufacture a molecular beam epitaxy crucible, and the method comprises the following steps:
[0008] S1. Prepare a graphite mandrel assembly;
[0009] S2, epitaxially depositing a first pyrolytic boron nitride layer on the periphery of the mandrel assembly;
[0010] S3, bending and winding a heating wire around the outer periphery of the first pyrolytic boron nitride layer so that the heating wire is closely fixed on the surface of the first pyrolytic boron nitride layer;
[0011] S4, epitaxially depositing a second pyrolytic boron nitride layer on the periphery of the first pyrolytic boron nitride layer, wherein the second pyrolytic boron nitride layer completely covers the heating wire;
[0012] S5. Oxidation eliminates the mandrel assembly.
[0013] Compared with the traditional epitaxial crucible manufacturing process, the integrated molecular beam epitaxial crucible manufacturing method of the present application divides the preparation process of the pyrolytic boron nitride layer into two stages, and between the two stages, the heating wire originally arranged outside the pyrolytic boron nitride layer is arranged inside the pyrolytic boron nitride layer, so that the molecular beam epitaxial crucible obtained has a heating wire that is completely covered by the pyrolytic boron nitride layer, which effectively simplifies the manufacturing process of the molecular beam epitaxial crucible and makes the manufactured molecular beam epitaxial crucible have the characteristics of simple structure and low manufacturing cost.
[0014] The integrated molecular beam epitaxy crucible manufacturing method, wherein the mandrel assembly comprises a substrate and a column, and the column is detachably mounted on one end of the substrate;
[0015] Step S5 includes:
[0016] S51, removing the column on the base, so that the base has exposed column holes;
[0017] S52, introducing an oxidizing gas into the column holes to gradually oxidize and eliminate the matrix.
[0018] The integrated molecular beam epitaxy crucible manufacturing method of the present application is based on removing the column in step S51 so that the column holes on the substrate are exposed to the oxidizing gas during the treatment in step S52, thereby increasing the contact area between the oxidizing gas and the substrate to improve the oxidation elimination efficiency, so that the oxidizing gas can continue to oxidize along the column holes to the surrounding areas, that is, the oxidation elimination efficiency inside the substrate is improved.
[0019] In the method for manufacturing an integrated molecular beam epitaxy crucible, the oxidizing gas is air and the oxidation temperature is 700-800°C.
[0020] In the integrated molecular beam epitaxial crucible manufacturing method, the first pyrolytic boron nitride layer and the second pyrolytic boron nitride layer are both formed by reaction deposition of gaseous boron trichloride and ammonia under high temperature conditions.
[0021] The integrated molecular beam epitaxy crucible manufacturing method further includes the following steps between step S2 and step S3:
[0022] S2', cooling the mandrel assembly having the first pyrolytic boron nitride layer to room temperature according to a cooling time of 12-24 hours.
[0023] In this example, the first pyrolytic boron nitride layer is cooled to room temperature according to a cooling time of 12-24 hours. The core shaft assembly and the first pyrolytic boron nitride layer can be cooled at the smallest possible cooling rate to reduce deformation and shrinkage detachment problems caused by differences in material shrinkage rates, thereby ensuring that the first pyrolytic boron nitride layer obtained after cooling is still tightly attached to the outer surface of the core shaft assembly.
[0024] The integrated molecular beam epitaxy crucible manufacturing method, wherein the thickness of the first pyrolytic boron nitride layer is 0.8-1.2 mm, and the thickness of the second pyrolytic boron nitride layer is greater than or equal to the first pyrolytic boron nitride layer.
[0025] In the method for manufacturing an integrated molecular beam epitaxy crucible, the mandrel assembly is cylindrical, and step S3 comprises:
[0026] S31, bending the heating wire into a circular ring shape with an outer diameter smaller than the outer diameter of the first pyrolytic boron nitride layer;
[0027] S32, stretching and sleeve-fitting the bent heating wire onto the outer periphery of the first pyrolytic boron nitride layer.
[0028] The integrated molecular beam epitaxy crucible manufacturing method, wherein, in step S31, the bending radius of the heating wire is 1-2 mm.
[0029] In a second aspect, the present application further provides an epitaxial crucible, which is manufactured based on the integrated molecular beam epitaxial crucible manufacturing method provided in the first aspect.
[0030] The epitaxial crucible of the present application integrates the heating wire into the pyrolytic boron nitride layer, so that the heating wire is no longer exposed to the external environment. It has the characteristics of simple structure, low production cost, high production efficiency, high thermal efficiency, uniform thermal field distribution and outstanding thermal insulation effect.
[0031] In a third aspect, the present application further provides a molecular beam source furnace, comprising an epitaxial crucible manufactured based on the integrated molecular beam epitaxial crucible manufacturing method provided in the first aspect.
[0032] The molecular beam source furnace of the present application is provided with an integrated epitaxial crucible, which integrates the heating wire into the pyrolytic boron nitride layer, so that the heating wire is no longer exposed to the external environment, so that the molecular beam source furnace of the present application has the characteristics of simple structure, low production cost, high production efficiency, high thermal efficiency, uniform thermal field distribution and outstanding thermal insulation effect.
[0033] As can be seen from the above, the present application provides an integrated molecular beam epitaxy crucible manufacturing method, an epitaxial crucible and a molecular beam source furnace, wherein the manufacturing method divides the preparation process of the pyrolytic boron nitride layer into two stages, and between the two stages, the heating wire originally arranged outside the pyrolytic boron nitride layer is arranged inside the pyrolytic boron nitride layer, so that the molecular beam epitaxial crucible obtained by manufacturing has a heating wire that is completely covered by the pyrolytic boron nitride layer, that is, the installation and fixation of the heating wire is completed by using the pyrolytic boron nitride layer, which effectively simplifies the manufacturing process of the molecular beam epitaxy crucible, so that the manufactured molecular beam epitaxy crucible has the characteristics of simple structure and low manufacturing cost; in addition, the integrated molecular beam epitaxy crucible manufacturing method of the present application realizes the manufacturing of the integrated molecular beam epitaxy crucible by changing the process sequence and reconstructing the structure of the molecular beam epitaxy crucible, that is, without adding additional process means, an integrated molecular beam epitaxy crucible with simple structure, low manufacturing cost, high manufacturing efficiency, high thermal efficiency, uniform thermal field distribution and outstanding thermal insulation effect can be manufactured. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the structure of a molecular beam source furnace in the prior art.
[0035] Figure 2 This is a flow chart of a method for manufacturing an integrated molecular beam epitaxy crucible provided in an embodiment of the present application.
[0036] Figure 3 It is a schematic diagram of the processing flow of step S2 to step S4.
[0037] Figure 4 It is a structural schematic diagram of the core shaft assembly.
[0038] Figure 5 A schematic diagram of the structure of an epitaxial crucible provided in an embodiment of the present application.
[0039] Figure numerals: 101, crucible; 102, hot wire assembly; 103, temperature measuring thermocouple; 104, side shielding cover; 105, top shielding cover; 106, bottom shielding cover; 107, support base; 108, mounting flange; 109, heater feedthrough; 110, thermocouple feedthrough; 201, column; 202, substrate; 203, first pyrolytic boron nitride layer; 204, heating wire; 205, second pyrolytic boron nitride layer. DETAILED DESCRIPTION
[0040] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0041] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0042] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0043] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0044] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0045] like Figure 1 The figure shows an existing molecular beam source furnace. The traditional molecular beam source furnace includes a crucible 101, a heating wire assembly 102, a temperature measuring thermocouple 103, a side shielding cover 104, a top shielding cover 105, a bottom shielding cover 106, a support base 107, a mounting flange 108, a heater feedthrough 109 and a thermocouple feedthrough 110.
[0046] The heating wire assembly 102 of the molecular beam source furnace is not in contact with the crucible 101, and heat is mainly transferred to the crucible 101 by the form of radiation heat transfer of the heating wire assembly 102 itself for heating. Since the heating wire assembly 102 also radiates heat toward the side shielding cover 104, some heat loss will be caused, resulting in a low overall thermal efficiency of the molecular beam source furnace. In addition, the manufacturing process of the heating wire assembly 102 of the molecular beam source furnace is complicated, and the heating wire needs to be passed through the corresponding small holes on the support ring (an annular bracket installed on the support seat 107 for fixing the heating wire, which is combined with the heating wire to form the heating wire assembly 102) one by one for winding. A too small bending radius will cause the heating wire to bend and deform, increase the difficulty of winding, and also cause an uneven thermal field.
[0047] First, please refer to Figure 2-Figure 4 Some embodiments of the present application provide a method for manufacturing an integrated molecular beam epitaxy crucible, which is used to manufacture a molecular beam epitaxy crucible. The method includes the following steps:
[0048] S1. Prepare a graphite mandrel assembly;
[0049] S2, epitaxially depositing a first pyrolytic boron nitride layer 203 on the periphery of the mandrel assembly;
[0050] S3, bending and winding the heating wire 204 around the first pyrolytic boron nitride layer 203, so that the heating wire 204 is closely fixed on the surface of the first pyrolytic boron nitride layer 203;
[0051] S4, epitaxially depositing the second pyrolytic boron nitride layer 205 on the periphery of the first pyrolytic boron nitride layer 203, wherein the second pyrolytic boron nitride layer 205 completely covers the heating wire 204;
[0052] S5. Oxidation elimination mandrel assembly.
[0053] Specifically, the mandrel assembly is a base for making a molecular beam epitaxial crucible with a specific shape, that is, the specific shape and size of the mandrel assembly should be designed according to the shape and size of the molecular beam epitaxial crucible to be made.
[0054] More specifically, the mandrel assembly is made of graphite material, ensuring that step S5 can successfully remove the mandrel assembly completely to retain the molecular beam epitaxial crucible composed of the first pyrolytic boron nitride layer 203 , the heating wire 204 and the second pyrolytic boron nitride layer 205 .
[0055] More specifically, the first pyrolytic boron nitride layer 203 and the second pyrolytic boron nitride layer 205 are both hard layers. In step S3, the heating wire 204 is bent and wound around the first pyrolytic boron nitride layer 203 to preliminarily fix the heating wire 204 on the first pyrolytic boron nitride layer 203 by utilizing the contact friction between the heating wire 204 and the first pyrolytic boron nitride layer 203. In step S4, the second pyrolytic boron nitride layer 205 deposited will be connected to the first pyrolytic boron nitride layer 203 to form an integral pyrolytic boron nitride layer, and the preliminarily fixed heating wire 204 will be completely fixed. The heating wire 204 is completely fixed inside the pyrolytic boron nitride layer, so that the heating wire 204 is integrated in the epitaxial crucible, forming a similar embedded installation structure, and each part of the heating wire 204 is in close contact with the pyrolytic boron nitride layer, and can transfer the heat generated by itself to the pyrolytic boron nitride layer by contact heat transfer, thereby effectively improving the thermal efficiency and thermal field uniformity of the epitaxial crucible, and avoiding the heat of the heating wire 204 from radiating outward, so that the second pyrolytic boron nitride layer 205 can be used as a thermal insulation layer of the heating wire 204 to improve the thermal insulation effect of the epitaxial crucible.
[0056] More specifically, after the heating wire 204 is bent and wound, its shape is fixed by the second pyrolytic boron nitride layer 205, which can prevent the heating wire 204 from being deformed or displaced relative to the pyrolytic boron nitride layer, so that the epitaxial crucible does not need to use a fixing clamp such as a support ring to install and fix the heating wire 204, effectively reducing the installation difficulty of the heating wire 204 and reducing the installation cost.
[0057] More specifically, both step S2 and step S4 utilize epitaxial deposition to generate corresponding pyrolytic boron nitride layers, ensuring that the corresponding layer structure has uniform circumferential density and thickness along the periphery of the core shaft assembly, thereby ensuring that the thermal field generated by the epitaxial crucible is uniform when in use.
[0058] More specifically, during the manufacturing process, the heating wire 204 is fixed tightly on the surface of the first pyrolytic boron nitride layer 203 by bending and winding. The shape of the heating wire 204 can be adjusted online according to factors such as heating setting requirements to adjust the thermal field distribution, that is, the distribution density, position, etc. of the heating wire 204 can be freely adjusted until the design requirements are met, and then step S4 is used to completely fix the heating wire 204.
[0059] Compared with the traditional epitaxial crucible manufacturing process, the integrated molecular beam epitaxial crucible manufacturing method of the embodiment of the present application divides the preparation process of the pyrolytic boron nitride layer into two stages, and between the two stages, the heating wire 204 originally arranged outside the pyrolytic boron nitride layer is arranged inside the pyrolytic boron nitride layer, so that the molecular beam epitaxial crucible obtained by manufacturing has a heating wire 204 that is completely covered by the pyrolytic boron nitride layer, that is, the installation and fixation of the heating wire 204 is completed by using the pyrolytic boron nitride layer, which effectively simplifies the manufacturing process of the molecular beam epitaxial crucible, so that the manufactured molecular beam epitaxial crucible has the characteristics of simple structure and low manufacturing cost; in addition, the integrated molecular beam epitaxial crucible manufacturing method of the embodiment of the present application realizes the manufacturing of the integrated molecular beam epitaxial crucible by changing the process sequence and reconstructing the molecular beam epitaxial crucible structure, that is, without adding additional process means, an integrated molecular beam epitaxial crucible with simple structure, low manufacturing cost, high manufacturing efficiency, high thermal efficiency, uniform thermal field distribution and outstanding thermal insulation effect can be manufactured.
[0060] In some preferred embodiments, the mandrel assembly includes a base 202 and a column 201, wherein the column 201 is detachably mounted on one end of the base 202;
[0061] Step S5 includes:
[0062] S51, removing the column 201 on the base 202, so that the base 202 has an exposed column hole;
[0063] S52, introducing an oxidizing gas into the column holes to gradually oxidize and eliminate the substrate 202.
[0064] It should be understood that the first pyrolytic boron nitride layer 203 and the second pyrolytic boron nitride layer 205 deposited in step S2 and step S4 also cover the end of the substrate 202 away from the column 201, and this part of the layer constitutes the bottom of the molecular beam epitaxy crucible, so that the oxidizing gas can only enter from the end of the substrate 202 with the column hole.
[0065] Specifically, the base 202 and the column 201 in the mandrel assembly are both manufactured by turning, and both are made of graphite, wherein the base 202 is preferably made of fine-grained, high-density, pre-refined graphite, and the column 201 is preferably made of extruded graphite with high hardness and coarse particles; steps S2 to S4 all need to be performed when the installation position of the mandrel assembly is fixed. The mandrel assembly generally uses a clamp to fix the column 201 to fix the installation position. Therefore, the column 201 made of extruded graphite with high hardness and coarse particles can ensure that the mandrel assembly is firmly fixed.
[0066] More specifically, the column 201 is detachably mounted in a column hole on the base 202. The column hole may be in the form of a stepped hole, a threaded hole, a countersunk hole, etc. To ensure that the column 201 can be firmly mounted on the base 202, in an embodiment of the present application, the column hole is preferably a threaded hole so that the column 201 can be threadedly connected to the base 202.
[0067] More specifically, the graphite substrate 202 can be oxidized and eliminated using an oxidizing gas, and the elimination efficiency of the substrate 202 can be accelerated under appropriate heating conditions; the integrated molecular beam epitaxy crucible manufacturing method of the embodiment of the present application is based on step S51 to remove the column 201 so that the column holes on the substrate 202 are exposed to the oxidizing gas during the treatment process of step S52, thereby increasing the contact area between the oxidizing gas and the substrate 202 to improve the oxidation elimination efficiency, so that the oxidizing gas can continue to oxidize along the column holes to the surrounding areas, that is, the oxidation elimination efficiency inside the substrate 202 is improved.
[0068] The epitaxial crucible is generally cylindrical, therefore, in some preferred embodiments, the substrate 202 is preferably cylindrical, so that the first pyrolytic boron nitride layer 203 and the second pyrolytic boron nitride layer 205 deposited on the outer peripheral surface of the substrate 202 in step S2 and step S4 are both cylindrical.
[0069] More specifically, in order to limit the growth boundary of the first pyrolytic boron nitride layer 203 and the second pyrolytic boron nitride layer 205, the substrate 202 has a circumferentially protruding rib near the end face of the column 201, and the rib is used to limit the growth position of the first pyrolytic boron nitride layer 203 and the second pyrolytic boron nitride layer 205; it should be understood that after the deposition reaction of step S2 and step S4 or after the end of step S5, the edge material deposited on the rib needs to be removed by cutting or grinding process to ensure that the edge of the molecular beam epitaxy crucible is flush.
[0070] In some preferred embodiments, the oxidizing gas is air and the oxidation temperature is 700-800°C.
[0071] Specifically, considering the oxidation conditions of the graphite material and the oxygen content in the air, the oxidation treatment process in step S5 should be above 300° C. Properly increasing the oxidation treatment temperature can increase the oxidation treatment efficiency.
[0072] More specifically, since the oxidation temperature of the pyrolytic boron nitride layer is about 1000°C (1273K), the pyrolytic boron nitride layer must be prevented from being oxidized during the oxidation process of the graphite substrate 202. Therefore, in the embodiment of the present application, the oxidation temperature is set below 1000°C, preferably 700-800°C, to ensure that the substrate 202 can be efficiently oxidized and eliminated and to avoid the pyrolytic boron nitride layer being affected.
[0073] More specifically, in the embodiment of the present application, air is used as the oxidizing gas to eliminate the substrate 202, which can effectively reduce the oxidation cost.
[0074] In some preferred embodiments, the first pyrolytic boron nitride layer 203 and the second pyrolytic boron nitride layer 205 are both formed by reaction deposition of gaseous boron trichloride and ammonia under high temperature conditions.
[0075] Specifically, the reaction formula of gaseous boron trichloride and ammonia under high temperature conditions is:
[0076] BCl 3 (g) + NH 3 (g) = BN(s) + 3HCl(g);
[0077] The pyrolytic boron nitride layer is made by dropping small hexagonal boron nitride snowflakes one by one in parallel onto the graphite substrate 202 material and then cooling and demolding.
[0078] More specifically, it should be understood that both step S2 and step S4 perform deposition reactions in an epitaxial growth chamber of a chemical vapor deposition reaction, by introducing gaseous boron trichloride and ammonia into the epitaxial growth chamber to react and generate a first pyrolytic boron nitride layer 203 deposited on the core shaft assembly and a second pyrolytic boron nitride layer 205 deposited on the first pyrolytic boron nitride layer 203.
[0079] More specifically, in the embodiment of the present application, during the reaction process in the epitaxial growth chamber, in addition to introducing gaseous boron trichloride and ammonia, a diluent is also introduced as a carrier gas to control the reaction rate; in the embodiment of the present application, the diluent is preferably nitrogen.
[0080] More specifically, the high temperature condition is above 1700° C., that is, both step S2 and step S4 require that the epitaxial growth chamber be heated to 1700° C. before gaseous boron trichloride, ammonia and diluent are injected into the growth chamber for reaction deposition.
[0081] In some preferred embodiments, the following steps are further included between step S2 and step S3:
[0082] S2', cooling the mandrel assembly with the first pyrolytic boron nitride layer 203 to room temperature according to a cooling time of 12-24 hours.
[0083] Specifically, it can be seen from the foregoing that pyrolytic boron nitride is formed after the boron nitride is cooled. Since the layer generated by epitaxial deposition is a film structure, the thermal shrinkage rate of the first pyrolytic boron nitride layer 203 of the film structure is smaller than the thermal shrinkage rate of the general boron nitride material. If the cooling rate is too fast, it is easy to cause the layer structure to have a morphological change problem due to uneven thermal shrinkage rate, and the core shaft assembly may shrink and detach from the first pyrolytic boron nitride layer 203, resulting in a gap between the two, thereby affecting the epitaxial deposition effect of step S4; therefore, in the embodiment of the present application, a slow cooling method is used to cool the first pyrolytic boron nitride layer 203, that is, the first pyrolytic boron nitride layer 203 is cooled to room temperature according to 12-24 hours, that is, the core shaft assembly and the first pyrolytic boron nitride layer 203 are cooled at the smallest possible cooling rate to reduce the deformation and shrinkage and detachment problems caused by the difference in material shrinkage rates, thereby ensuring that the first pyrolytic boron nitride layer 203 obtained after cooling is still tightly attached to the outer surface of the core shaft assembly.
[0084] More specifically, the mandrel assembly and the first pyrolytic boron nitride layer 203 obtained after the cooling process need to be taken out of the growth chamber for winding the heating wire 204 .
[0085] In some preferred embodiments, the first pyrolytic boron nitride layer 203 has a thickness of 0.8-1.2 mm, and the second pyrolytic boron nitride layer 205 has a thickness greater than or equal to that of the first pyrolytic boron nitride layer 203 .
[0086] Specifically, in the application embodiment, the first pyrolytic boron nitride layer 203 is preferably 1 mm.
[0087] More specifically, in step S2, 6 L / min of high-purity nitrogen, 0.6 L / min of boron trichloride, and 1 L / min of ammonia are introduced into the growth chamber, and reaction deposition is performed at 1700°C for 18-24 hours, so that a first pyrolytic boron nitride layer 203 with a thickness of 0.8-1 mm can be generated on the outer surface of the core shaft assembly. The first pyrolytic boron nitride layer 203 is attached to the outer surface of the core shaft assembly in the form of a pyrolytic boron nitride film.
[0088] More specifically, in the embodiment of the present application, the heating wire 204 is preferably a tantalum heating wire, and the cross-sectional diameter of the tantalum heating wire is generally 0.8 mm. Therefore, the thickness of the second pyrolytic boron nitride layer 205 is designed to be greater than or equal to the first pyrolytic boron nitride layer 203 to ensure that the second pyrolytic boron nitride layer 205 completely covers the heating wire 204.
[0089] More specifically, in the embodiment of the present application, the second pyrolytic boron nitride layer 205 is preferably 1.8 mm, so that the portion of the second pyrolytic boron nitride layer 205 higher than the heating wire 204 has a thickness of 1 mm, so that the heating wire 204 is located in the middle position of the pyrolytic boron nitride layer of the integrated molecular beam epitaxy crucible finally obtained.
[0090] In some preferred embodiments, the mandrel assembly is cylindrical, and step S3 comprises:
[0091] S31, bending the heating wire 204 into a circular ring shape with an outer diameter smaller than the outer diameter of the first pyrolytic boron nitride layer 203;
[0092] S32 , stretching and sleeve-fitting the bent heating wire 204 onto the outer periphery of the first pyrolytic boron nitride layer 203 .
[0093] Specifically, it can be known from the above content that the core shaft assembly includes a cylindrical base 202, so it is cylindrical as a whole.
[0094] More specifically, in the embodiment of the present application, the heating wire 204 is bent based on a serpentine bending manner to form a circular ring structure that can evenly cover the outer periphery of the first pyrolytic boron nitride layer 203 .
[0095] More specifically, in the embodiment of the present application, the outer diameter of the circular ring structure of the heating wire 204 is slightly smaller than the outer diameter of the cylindrical first pyrolytic boron nitride layer 203, so that the heating wire 204 can be sleeved on the outer periphery of the first pyrolytic boron nitride layer 203 under a slight stretching effect, and is tightly fixed to the outer periphery of the first pyrolytic boron nitride layer 203 based on the elastic potential energy generated by its own stretching.
[0096] More specifically, in some other embodiments, the heating wire 204 is bent based on another core shaft assembly, so that the heating wire 204 with a circular ring structure fits the shape of the core shaft assembly and the outer diameter of its circular ring structure is slightly smaller than the outer diameter of the cylindrical first pyrolytic boron nitride layer 203, and can be sleeved and fixed on the first pyrolytic boron nitride layer 203; in this embodiment, the shape of the heating wire 204 is adjusted based on the core shaft assembly, which can simplify the bending processing process of the heating wire 204.
[0097] More specifically, the annular heating wire 204 has good expansion elasticity. When the heating wire 204 is sleeved on the periphery of the first pyrolytic boron nitride layer 203, appropriate stretching adjustment can be performed to ensure that the heating wire 204 is evenly distributed on the periphery of the first pyrolytic boron nitride layer 203, thereby ensuring the thermal field uniformity of the molecular beam epitaxy crucible.
[0098] More specifically, it should be understood that after the processing in step S32, the heating wire 204 has a lead extending from one end of the first pyrolytic boron nitride layer 203, and the lead is used to connect the heater of the epitaxial crucible; in the embodiment of the present application, step S3 also includes:
[0099] S33, fixing the lead wire of the heating wire 204 using a fixture.
[0100] More specifically, after the heating wire 204 is installed and fixed, using a fixture to fix the lead wire of the heating wire 204 can achieve a better fixing effect of the heating wire 204, and effectively avoid problems such as displacement of the heating wire 204 during the processing of step S4.
[0101] More specifically, there are one or more heating wires 204 of a circular ring structure, and the specific number and size of the heating wires 204 can be selected according to the number and length of the temperature zones of the molecular beam epitaxy crucible.
[0102] In some preferred embodiments, in step S31, the bending radius of the heating wire 204 is 1-2 mm, which can avoid the short circuit of the heating wire 204 and ensure uniform thermal field distribution of the molecular beam epitaxy crucible.
[0103] Second, please refer to Figure 5 Some embodiments of the present application further provide an epitaxial crucible, which is made based on the integrated molecular beam epitaxial crucible manufacturing method provided in the first aspect.
[0104] Specifically, the epitaxial crucible includes an integral cylindrical pyrolytic boron nitride layer, in which a uniformly bent and wound heating wire 204 is built. The heating wire 204 is completely covered by the pyrolytic boron nitride layer, and only has a lead end extending from one side of the pyrolytic boron nitride layer.
[0105] The epitaxial crucible of the embodiment of the present application integrates the heating wire 204 into the pyrolytic boron nitride layer, so that the heating wire 204 is no longer exposed to the external environment. It has the characteristics of simple structure, low production cost, high production efficiency, high thermal efficiency, uniform heat field distribution and outstanding thermal insulation effect.
[0106] In addition, since the heating wire 204 is arranged inside the pyrolytic boron nitride layer, the evaporation material will not condense and adhere to the surface of the heating wire 204 during epitaxial growth in the epitaxial crucible, thereby preventing the evaporation material from causing the thermal effect of the heating wire 204 to decay or even short-circuit.
[0107] In a third aspect, some embodiments of the present application further provide a molecular beam source furnace, comprising an epitaxial crucible manufactured based on the integrated molecular beam epitaxial crucible manufacturing method provided in the first aspect.
[0108] Specifically, the molecular beam source furnace is a structure modification of the epitaxial crucible in the existing molecular beam source furnace, so that the heating wire 204 originally located outside the epitaxial crucible is integrated into the pyrolytic boron nitride layer, and the support seat, mounting flange, heater feedthrough and thermocouple feedthrough and other devices can still be connected to the epitaxial crucible using traditional installation methods.
[0109] More specifically, since the heating wire 204 is integrated in the pyrolytic boron nitride layer, the pyrolytic boron nitride layer can play a heat-insulating effect. Therefore, the molecular beam source furnace in the embodiment of the present application can abandon the shielding layer originally arranged on the outside of the epitaxial crucible, or use a shielding layer with a smaller thickness to further save the structural cost of the molecular beam source furnace.
[0110] The molecular beam source furnace of the embodiment of the present application is provided with an integrated epitaxial crucible, which integrates the heating wire 204 in the pyrolytic boron nitride layer, so that the heating wire 204 is no longer exposed to the external environment, so that the molecular beam source furnace of the embodiment of the present application has the characteristics of simple structure, low production cost, high production efficiency, high thermal efficiency, uniform thermal field distribution and outstanding thermal insulation effect.
[0111] In summary, the embodiments of the present application provide an integrated molecular beam epitaxy crucible manufacturing method, an epitaxial crucible and a molecular beam source furnace, wherein the manufacturing method divides the preparation process of the pyrolytic boron nitride layer into two stages, and between the two stages, the heating wire 204 originally arranged in the air outside the pyrolytic boron nitride layer is arranged inside the pyrolytic boron nitride layer, so that the molecular beam epitaxial crucible obtained by manufacturing has a heating wire 204 that is completely covered by the pyrolytic boron nitride layer, that is, the installation and fixation of the heating wire 204 is completed by using the pyrolytic boron nitride layer, which effectively simplifies the manufacturing process of the molecular beam epitaxy crucible, so that the manufactured molecular beam epitaxy crucible has the characteristics of simple structure and low manufacturing cost; in addition, the integrated molecular beam epitaxy crucible manufacturing method of the embodiment of the present application realizes the manufacturing of the integrated molecular beam epitaxy crucible by changing the process sequence and reconstructing the molecular beam epitaxy crucible structure, that is, without adding additional process means, an integrated molecular beam epitaxy crucible with simple structure, low manufacturing cost, high manufacturing efficiency, high thermal efficiency, uniform thermal field distribution and outstanding thermal insulation effect can be manufactured.
[0112] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0113] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for manufacturing an integrated molecular beam epitaxy crucible, for manufacturing a molecular beam epitaxy crucible, characterized in that: The method comprises the following steps: S1. Prepare a graphite mandrel assembly; S2, epitaxially depositing a first pyrolytic boron nitride layer on the periphery of the mandrel assembly; S3, bending and winding a heating wire around the outer periphery of the first pyrolytic boron nitride layer so that the heating wire is closely fixed on the surface of the first pyrolytic boron nitride layer; S4, epitaxially depositing a second pyrolytic boron nitride layer on the periphery of the first pyrolytic boron nitride layer, wherein the second pyrolytic boron nitride layer completely covers the heating wire; S5, oxidizing and eliminating the mandrel assembly; The mandrel assembly is cylindrical, and step S3 comprises: S31, bending the heating wire into a circular ring shape with an outer diameter smaller than the outer diameter of the first pyrolytic boron nitride layer; S32, stretching and sleeve-fitting the bent heating wire onto the outer periphery of the first pyrolytic boron nitride layer; S33, fixing the lead of the heating wire based on the fixture; The spindle assembly comprises a base and a column, wherein the column is detachably mounted on one end of the base; Step S5 includes: S51, removing the column on the base, so that the base has exposed column holes; S52, introducing an oxidizing gas into the column holes to gradually oxidize and eliminate the matrix.
2. The method for manufacturing an integrated molecular beam epitaxy crucible according to claim 1, characterized in that: The oxidizing gas is air, and the oxidizing temperature is 700-800°C.
3. The method for manufacturing an integrated molecular beam epitaxy crucible according to claim 1, characterized in that: The first pyrolytic boron nitride layer and the second pyrolytic boron nitride layer are both formed by reaction deposition of gaseous boron trichloride and ammonia under high temperature conditions.
4. The method for manufacturing an integrated molecular beam epitaxy crucible according to claim 1, characterized in that: The following steps are also included between step S2 and step S3: S2', cooling the mandrel assembly having the first pyrolytic boron nitride layer to room temperature according to a cooling time of 12-24 hours.
5. The method for manufacturing an integrated molecular beam epitaxy crucible according to claim 1, characterized in that: The thickness of the first pyrolytic boron nitride layer is 0.8-1.2 mm, and the thickness of the second pyrolytic boron nitride layer is greater than or equal to the first pyrolytic boron nitride layer.
6. The method for manufacturing an integrated molecular beam epitaxy crucible according to claim 1, characterized in that: In step S31, the bending radius of the heating wire is 1-2 mm.
7. An epitaxial crucible, characterized in that: The epitaxial crucible is made based on the integrated molecular beam epitaxial crucible manufacturing method according to any one of claims 1 to 6.
8. A molecular beam source furnace, characterized in that: It comprises an epitaxial crucible made based on the method for making an integrated molecular beam epitaxial crucible as described in any one of claims 1 to 6.