An activation method and application of optimized mechanically activated starch inhibitor

By adjusting the planetary milling parameters and SPSS fitting to determine the optimal charging conditions, and preparing highly active starch inhibitors, the application of mechanically activated starch in mineral flotation is solved, and the sorting efficiency and starch performance are improved.

CN115646656BActive Publication Date: 2024-11-15WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211225872.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-09
Publication Date
2024-11-15
Estimated Expiration
2042-10-09

AI Technical Summary

Technical Problem

The prior art does not clarify the impact of mechanical activation methods on the ability of starch molecules to inhibit mineral flotation, and there is no application of mechanically activated modified starch in the field of mineral flotation, which is difficult to meet the modern industry's demand for improving starch performance.

Method used

By adjusting the mechanical activation parameters of the planetary mill, mechanically activated starch inhibitors under different conditions are prepared, charging energy values ​​are calculated, and recovery-energy formulas are obtained through SPSS fitting, the optimal charging energy values ​​and parameters are determined, and the preparation Highly active starch inhibitors to improve mineral sorting efficiency.

Benefits of technology

The quality control of starch inhibitors is achieved, its ability to act in mineral flotation is improved, gelatinization temperature and coagulation are reduced, and sorting efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115646656B_ABST
    Figure CN115646656B_ABST
Patent Text Reader

Abstract

The invention discloses an activation method and application of an optimized mechanically activated starch inhibitor, comprising the following steps: S1. using starch as a raw material, charging the starch raw material by adjusting a set of mechanical activation parameters, obtaining a mechanically activated starch inhibitor under different parameter conditions, and calculating the charging energy value of each mechanically activated starch inhibitor by a charging energy formula (I), #imgabs0# S2. using the mechanically activated starch as an inhibitor, performing flotation experiments on minerals respectively, and recording the flotation recovery rate; S3. fitting the corresponding charging energy value and flotation recovery rate by SPSS, obtaining the recovery rate-charging formula (II), ε=αE 2 +βE+γ(Ⅱ); S4. Calculate the charging energy value E through the recovery rate-charging formula (Ⅱ) i , E i The mechanical activation parameter set is brought into the charging energy formula (I), and the starch inhibitor prepared by using the determined parameters has strong reaction activity and high efficiency in inhibiting mineral flotation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral processing, and in particular to an activation method and application of an optimized mechanically activated starch inhibitor. Background Art

[0002] There are limited varieties of natural starch, and there are disadvantages such as insolubility in cold water, poor thermal stability of the paste, low shear resistance, easy dehydration after cooling, easy aging, poor film-forming properties and lack of water resistance. At the same time, the application scope is limited under the circumstances of the widespread use of new processes, new equipment and new technologies in modern industry, and it can no longer meet the needs of the increasingly developed modern processes and equipment. Therefore, it is necessary to modify the starch.

[0003] Starch modification is the use of physical, chemical or biological means to change the properties of natural starch. Starch derivatives with changed properties, i.e. modified starch, can be obtained by molecular cutting, rearrangement, oxidation or introducing substituents into starch molecules. This is used to increase its performance or introduce new properties, overcome defects in application, and meet the needs of modern industrial production. Physical means include mechanical activation, which refers to the process in which an object will produce lattice distortion and local damage under the action of mechanical force, and form various defects, resulting in an increase in its internal energy and enhanced reaction activity.

[0004] As a natural macromolecular compound, starch is often used as an inhibitor in mineral flotation, that is, selectively inhibiting the flotation of certain minerals, expanding the floatability differences between different minerals, and improving the flotation efficiency. However, existing studies have not yet clarified the effect of mechanical activation methods on the ability of starch molecules to inhibit mineral flotation, nor have they applied mechanically activated modified starch in the field of mineral flotation. Therefore, it is necessary to explore the effect of mechanical activation conditions on the inhibitory ability of starch molecules, and to clarify the optimal process conditions for preparing starch inhibitors, so as to improve their separation efficiency in mineral flotation applications. Summary of the invention

[0005] In view of this, the present application provides an activation method and application of an optimized mechanically activated starch inhibitor, wherein the starch inhibitor prepared by the determined parameters has high activity and high mineral separation efficiency.

[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions:

[0007] In a first aspect, the present application provides a method for optimizing the activation of a mechanically activated starch inhibitor, comprising the following steps:

[0008] S1. Using starch as raw material, adjusting the mechanical activation parameter set of the planetary mill, performing dry mechanical activation solid phase reaction to charge the starch raw material, obtaining mechanically activated starch inhibitors under different parameter conditions, and calculating the charging energy value of each mechanically activated starch inhibitor;

[0009] S2. Using mechanically activated starch as an inhibitor, flotation experiments were performed on the minerals respectively, and the flotation recovery rates were recorded;

[0010] S3. Use SPSS to fit the corresponding charging energy value and flotation recovery rate to obtain the recovery rate-charging formula (Ⅱ),

[0011] ε=αE 2 +βE+γ(Ⅱ),

[0012] Where ε is the flotation recovery rate; α, β, and γ are constants determined by the type of starch;

[0013] S4. Calculate the optimal charging energy value E through the recovery rate-charging formula (Ⅱ) i , E i Substitute it into the charging energy formula (I) to reversely determine the optimal mechanical activation parameter set;

[0014] S5. Prepare a mechanically activated starch inhibitor based on the optimal mechanical activation parameter set.

[0015] Preferably, in step S4, the optimal charging energy value E i The calculation method is to take the derivative of the recovery rate-charging formula (II) and equal it to zero, and the extreme value is the optimal charging energy value E i .

[0016] Preferably, the starch raw material includes one or more of corn starch, potato starch, glutinous rice starch, rice starch and the like.

[0017] Preferably, in step S4, the mechanical activation parameter set includes three parameters: ball-to-material ratio, planetary mill speed, and activation time; the optimal charging energy value E i Substitute it into the charging energy formula (I), calculate the remaining parameter based on any two parameters in the mechanical activation parameter set, and record the obtained three parameters as the optimal mechanical activation parameter set.

[0018] Preferably, in step S1, the charging energy value ranges from 2.6KJ to 32KJ.

[0019] Preferably, the steps of the flotation experiment are: adding deionized water to the ore sample to be floated, adjusting the pH to alkaline, adding an aqueous solution of a mechanically activated starch inhibitor, stirring, and then adding a collector, stirring, flotation scraping, filtering the product in the tank, drying, and weighing to obtain the grade and recovery rate of the flotation concentrate.

[0020] Preferably, the charging energy value is calculated by the charging energy formula (I),

[0021]

[0022] Among them, E is the charging energy, f is the starch activation index, τ is the ball-to-material ratio, e i is the unit energy consumption of the planetary mill, N is the rotation speed of the planetary mill, and T is the activation time.

[0023] In a second aspect, the present application provides a mechanically activated starch inhibitor.

[0024] In a third aspect, the present application provides an application of a mechanically activated starch inhibitor in mineral separation.

[0025] Preferably, the minerals include one or more of hematite, barite, kaolinite and the like.

[0026] The beneficial effects of this application are as follows:

[0027] The charging energy formula and the recovery rate-charging formula in the present invention can control the quality of the starch inhibitor, obtain the finished mechanically activated starch with the best inhibitory effect, and determine the combination of the best input energy for the mechanically activated starch and the best mechanical activation conditions, thereby optimizing the preparation process of the starch inhibitor.

[0028] By adjusting the planetary milling time, number of revolutions and ball-to-material ratio through the method of the present invention, the obtained starch inhibitor is precisely controlled, and the starch is activated without destroying the internal structure of the starch, thereby increasing its solubility and reducing the gelatinization temperature and retrogradation of the starch.

[0029] The obtained starch inhibitor is used for mineral flotation. Due to the high reactivity of mechanically activated starch, its ability to interact with the surface of some minerals during flotation is effectively improved, making the mineral hydrophilic and hindering the binding of the collector, thereby selectively reducing the flotation recovery rate of some minerals and improving the sorting efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a comparison chart of the effect of corn starch inhibitor prepared under different mechanical activation time conditions on the flotation recovery rate of hematite;

[0031] Figure 2 This is a comparison chart of the effect of corn starch inhibitor on the flotation recovery rate of hematite under different planetary ball mill speed conditions;

[0032] Figure 3 This is a comparison chart of the effect of corn starch inhibitor prepared under different ball-to-material ratio conditions on the flotation recovery rate of hematite;

[0033] Figure 4 This is a functional relationship diagram of corn starch inhibitor recovery rate-energy charging formula;

[0034] Figure 5 This is the technical roadmap for this solution. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0036] Explanation of terms

[0037] "Starch activation index" refers to the conversion efficiency of different starches for mechanical activation energy, which is determined by the properties of each starch itself;

[0038] "Specific energy consumption of planetary mill" refers to the rated power of the selected planetary mill instrument;

[0039] “Charging energy” refers to the input energy obtained by converting starch raw materials into mechanical activity energy through the planetary mill.

[0040] As is well known to those skilled in the art, mechanical activation refers to a process in which an object undergoes lattice distortion and local damage under the action of mechanical force, and forms various defects, which results in an increase in its internal energy and an increase in its reactivity. With the continuous iteration of mechanical activation equipment, the control of the input energy of an object becomes more and more precise, easier to calculate, and convenient for simulation and fitting. Therefore, mechanical activation equipment can control the quality of the finished product of an object, which provides a way to obtain the most effective activated product and determine the optimal input energy for the object.

[0041] The applicant has found that mechanical activation can enhance the activity of starch hydroxyl functional groups and change and optimize the interaction structure between starch molecules and mineral surfaces, while excessive energy input will weaken the chain structure of starch molecules and greatly reduce their inhibitory ability. The formula obtained by data fitting can be used to reversely obtain the optimal activation parameters, control the quality of starch inhibitors, and obtain mechanically activated starch products with the best inhibitory effect. The optimal input energy and optimal mechanical activation conditions for mechanically activated starch can also be determined to optimize the preparation process of starch inhibitors.

[0042] Based on the above, the present invention has been created.

[0043] The present application provides an activation method for optimizing mechanically activated starch inhibitors, such as Figure 5 As shown, the following steps are included:

[0044] S1. Starch is taken as raw material, weighed and placed in a planetary mill zirconium oxide tank for standby use, the planetary mill parameters are set, and mechanical activation is performed: the planetary mill revolutions, time and ball-to-material ratio are adjusted to mechanically activate and charge the starch, and different starch inhibitors are prepared for standby use; the above mechanical activation process, i.e., the dry ball milling process, can charge the starch raw material, and according to different planetary mill parameters, the corresponding charging energy values ​​E1, E2, E3, E4, E5, E6... are calculated according to the charging energy formula (I),

[0045]

[0046] Among them, E is the charging energy, f is the starch activation index, τ is the ball-to-material ratio, e i is the unit energy consumption of the planetary mill, N is the rotation speed of the planetary mill, and T is the activation time;

[0047] S2. The starch inhibitor obtained is used as a solute and deionized water is used as a solvent to prepare a 0.8 g / L starch inhibitor solution; the starch inhibitor solution is used as an inhibitor to perform flotation separation on different minerals, including the following steps (taking hematite flotation as an example): 2 g hematite (200-400 mesh) is added to a flotation tank, 25 ml of deionized water is added and stirred for 2 min to form a slurry, the pH of the slurry is adjusted to 10, stirred for 2 min, an aqueous solution (2 ml) of a mechanically activated starch inhibitor is added to make the starch inhibitor concentration in the flotation tank 40 mg / L, after stirring for 2 min, 1 mL of a 1.6 g / L dodecylamine collector is added, stirred for 2 min, and 2 drops of a frother are added, and after flotation and scraping, the minerals in the tank are filtered, dried, and weighed, and the weighing data is recorded. The recovery rate is the mass ratio of the concentrate in the tank to the mass ratio of the weighed ore sample to be floated, and the corresponding mineral processing recovery rates ε1, ε2, ε3, ε4, ε5, ε6... are calculated;

[0048] S3. Collect the charging energy values ​​E1, E2, E3, E4, E5, E6... obtained under different parameter conditions in step S1, collect the mineral processing recovery rates ε1, ε2, ε3, ε4, ε5, ε6... of the starch inhibitors corresponding to the charging energy, perform SPSS fitting on the above data, and obtain the relationship between the charging energy value and the flotation recovery rate, i.e., the recovery rate-charging energy formula (II).

[0049] ε=αE 2 +βE+γ(Ⅱ),

[0050] Where ε is the flotation recovery rate; α, β, and γ are constants in the recovery rate-charging formula, which change with the change of starch;

[0051] S4. Calculate the optimal charging energy value E through the recovery rate-charging formula (Ⅱ) i , the best charging energy value E iThe calculation method is to take the derivative of the recovery rate-charging formula (II) and equal it to zero, and the extreme value is the optimal charging energy value E i , E i Substitute the charging energy formula (I) into the reverse calculation to determine the optimal mechanical activation parameter set. During the reverse calculation process, two of the three parameters are set to quantitative values ​​within the range to determine the value of the remaining parameter: the remaining parameter is calculated based on any two parameters in the mechanical activation parameter set, and the obtained three parameters are recorded as the optimal mechanical activation parameter set.

[0052] S5. Prepare a mechanically activated starch inhibitor based on the optimal mechanical activation parameter set.

[0053] In order to verify whether the theory matches the practical application, the starch inhibitor was prepared according to the appropriate mechanical activation conditions corresponding to this scheme, and the flotation experiment was carried out under the same conditions as in step S2 to test the flotation recovery rate and verify the accuracy of the recovery rate-charging formula. It was found that in this scheme, the goodness of fit of the energy charging formula and the recovery rate-charging formula were both greater than 0.9.

[0054] The charging energy formula (I) and recovery rate-charging formula (II) of this scheme provide theoretical support for the selection of preparation parameters of starch inhibitors, and play a vital role in the preparation process of starch inhibitors: first, to improve the quality of starch inhibitors and obtain mechanically activated starch products with the best inhibitory effect; second, to determine the optimal input energy of mechanically activated starch, select the optimal mechanical activation conditions accordingly, and optimize the preparation process of starch inhibitors. Mechanically activated starch can be used in the flotation of various minerals in the form of inhibitors to effectively separate the target minerals from the gangue minerals.

[0055] The starch raw materials include one or more of corn starch, potato starch, glutinous rice starch, rice starch, etc. Different starch raw materials correspond to different starch inhibitors. For example, through the above step S1, the corn starch (NS) raw material is subjected to dry mechanical activation solid phase reaction to obtain mechanically activated corn starch (NST), the glutinous rice starch (WS) raw material is subjected to dry mechanical activation solid phase reaction to obtain mechanically activated glutinous rice starch (WST), the G50 genetically modified corn starch is subjected to dry mechanical activation solid phase reaction to obtain mechanically activated G50 genetically modified corn starch (G50T), and the G80 genetically modified corn starch is subjected to dry mechanical activation solid phase reaction to obtain mechanically activated G80 genetically modified corn starch (G80T).

[0056] It is worth noting that in the charging energy formula (I), f is the starch activation constant, which refers to the conversion efficiency of different starches for mechanical activation charging, which is determined by the properties of each starch itself. For example, the starch constant f of ordinary corn is 1.26; e iis the unit energy consumption of the planetary mill, which is obtained by converting the power of the selected planetary mill instrument. In this application, the planetary mill used is the Pulverisette 6 series planetary ball mill of the German Flying Group, and its unit energy consumption is 1.2 J / c, and c is the number of revolutions of the planetary ball mill during operation; other parameters are variables, such as τ, N, and T. According to actual needs, the three are coordinated and adjusted. For example, in some specific embodiments, a zirconia jar with an inner diameter of 5 cm and a volume of 50 ml is selected, the diameter of the grinding balls in the ball mill is 1 cm, and the grinding balls are made of zirconia. In this solution, the rotation speed of the planetary mill is 200-600 r / min, and suitably but not restrictively, for example, 200 r / min, 300 r / min, 400 r / min, 500 r / min, 600 r / min, the ball-to-material ratio is 15:1, 20:1 or 30:1, and the activation time is 20:1. The time interval is 10-120min, and suitably but not restrictively, for example, 10min, 20min, 30min, 40min, 50min, 80min, 90min, 120min. Since the mechanical activation energy charging is too large and exceeds the threshold value that the starch can bear, the starch structure is destroyed, reducing the effect of the inhibitor. The mechanical activation energy charging is too low and the purpose of starch activation cannot be achieved. Therefore, in this scheme, the mechanical activation energy charging energy range determined by each mechanical activation condition is: 2.6KJ-32KJ. Based on the set mechanical activation energy charging range, the values ​​of the three variable parameters are adjusted, and the energy charging energy value E under different conditions is calculated by the energy charging energy formula (I);

[0057] Taking ordinary corn starch as an example, the recovery rate-energy charging formula obtained according to the above steps is: ε=0.002E 2 -0.043E+0.24, the extreme value is taken by the above formula, the flotation recovery rate is 1%, the energy E is 10.75KJ, the starch inhibitor has the best effect, that is, the optimal input energy of mechanically activated starch is 10.75KJ, and one of the optimal mechanical activation conditions that can be determined by the energy charging energy formula (I) is: speed 400r / min, activation time 20min, ball-to-material ratio 15:1. In order to verify the accuracy of the formula, the recovery rate-energy charging formula is obtained to determine the optimal input energy of mechanically activated starch, and a highly active starch inhibitor is obtained. The starch inhibitor is applied to the flotation experiment of hematite in this scheme. The hematite flotation recovery rate obtained at a low concentration of inhibitor is <1%, indicating that the formula provided by this method is highly accurate;

[0058] The present application provides a mechanically activated starch inhibitor.

[0059] The present application provides an application of a mechanically activated starch inhibitor in mineral sorting efficiency, wherein the minerals include one or more of hematite, barite, kaolinite, etc., so that the floatability of some minerals decreases to expand the floatability difference between different minerals, and the application steps are as follows: using the obtained starch inhibitor as a solute and deionized water as a solvent to prepare a 0.8 g / L starch inhibitor solution; using the above-mentioned starch inhibitor solution as an inhibitor to perform flotation separation on different minerals, comprising the following steps (taking hematite flotation as an example): adding 2 g of hematite (200-400 mesh) into a flotation tank, adding 25 ml of deionized water and stirring for 2 minutes to form a slurry, adjusting the pH of the slurry to 10, stirring for 2 minutes, adding an aqueous solution (2 ml) of a mechanically activated starch inhibitor to make the starch inhibitor concentration in the flotation tank 40 mg / L, stirring for 2 minutes, and then adding 1 mL 1.6g / L dodecylamine collector, stir for 2 minutes, then add 2 drops of frother, after flotation scraping, filter, dry and weigh the minerals in the tank, record the weighing data, the recovery rate is the mass ratio of the concentrate in the tank to the mass of the weighed ore sample to be floated, calculate the corresponding mineral processing recovery rate, and analyze the starch inhibitor effect.

[0060] The present solution is further described below in conjunction with specific embodiments.

[0061] Example 1

[0062] An activation method for optimizing mechanically activated starch inhibitors comprises the following steps:

[0063] S1. Preparation of mechanically activated starch inhibitor and calculation of charging energy

[0064] Weigh 4 g corn starch (NS) and place it in a planetary mill zirconia tank for later use;

[0065] The starch raw materials were dry-mechanically activated according to the planetary mill parameters set in experimental groups 1-5: with activation time as the variable, corn starch (NS) was mechanically activated for 10 min, 15 min, 25 min, 30 min, and 60 min at room temperature using a planetary mill at a speed of 400 r / min, and the ball-to-material ratio of grinding balls to corn starch (NS) was 15:1. After the mechanical ball milling process was completed, the corresponding charging energy value was calculated according to the charging energy formula (I):

[0066]

[0067] Among them, E is the charging energy, f is the starch activation index, τ is the ball-to-material ratio, e i is the unit energy consumption of the planetary mill, N is the rotation speed of the planetary mill, T is the activation time, f, e i is a constant, f is the activation index of corn starch (NS), which is 1.26, and e iis the unit energy consumption of the planetary mill, which is 1.2 J / c. According to the different ball-to-material ratios, activation time, and planetary mill speeds set in the experimental groups 1-5, different ordinary corn activated starch inhibitors were obtained, and the charging energies were calculated to be 5.376 KJ, 8.064 KJ, 13.44 KJ, 16.128 KJ, and 32.256 KJ of mechanically activated corn starch (NS), respectively. In this embodiment, the inner diameter of the zirconia tank is 4 cm and the volume is 50 ml; the diameter of the grinding balls in the zirconia tank is 1 cm, and the grinding ball material is zirconia.

[0068] S2. Flotation test, record experimental data

[0069] The different common corn activated starch inhibitors obtained in step S1 are subjected to a mineral flotation experiment and a recovery test is performed to obtain a recovery rate ε. The flotation experiment steps are as follows:

[0070] Weigh 0.08g starch and use deionized water as solvent to prepare a 0.8g / L starch inhibitor solution; use the starch inhibitor solution as an inhibitor to perform flotation separation on different minerals, including the following steps (taking hematite flotation as an example): add 2g hematite (200-400 mesh) into a flotation tank, add 25ml deionized water and stir for 2min to form a slurry, adjust the pH of the slurry to 10, stir for 2min, add an aqueous solution (2ml) of a mechanically activated starch inhibitor to make the starch inhibitor concentration in the flotation tank 40mg / L, stir for 2min, then add 1mL 1.6g / L dodecylamine collector, stir for 2min, then add 2 drops of a frother, scrape the flotation foam, filter, dry and weigh the minerals in the tank, record the weighing data, and the recovery rate is the mass ratio of the concentrate mass in the tank to the mass of the weighed ore sample to be floated, and the corresponding flotation recovery rate is calculated, and the results are as follows: Figure 1 shown.

[0071] S3. SPSS fits the recovery rate and charging data to obtain the recovery rate-charging formula

[0072] The parameters in step S1, the charging energy (E) calculated under different parameter conditions, and the flotation recovery rate (ε) recorded in step S2 are sorted out to obtain Table 1:

[0073] Table 1 Parameters of corn starch (NS) inhibitor

[0074] category Number of projects τ N(r / min) T(min) E(J) ε(%) Experimental Group 1 1 15 400 10 5376 19 Experimental Group 2 2 15 400 15 8064 9 Experimental Group 3 3 15 400 25 13440 8 Experimental Group 4 4 15 400 30 16128 16 Experimental Group 5 5 15 400 60 322560 22 Fitting the best group 6 15 400 20 10752 1

[0075] The charging energy (E) and flotation recovery (ε) in the above data were fitted by SPSS, and the results are as follows Figure 4 As shown in the figure, the fitting relationship between the inhibition recovery rate and the charging energy of ordinary corn activated starch is: ε=0.002E 2-0.043E+0.24, which is the recovery rate-charging formula of ordinary corn starch, and the goodness of fit R 2 =0.98, goodness of fit R 2 ≥0.9.

[0076] S4. Determine the optimal charging energy value E i and the optimal mechanical activation parameter set,

[0077] S5. Prepare a mechanically activated starch inhibitor based on the optimal mechanical activation parameter set.

[0078] By taking the derivative of the recovery rate-charging formula and taking the extreme value, the optimal charging energy value is 10750KJ. In this embodiment, only the activation time is a variable, and the ball-to-material ratio and the planetary mill speed are quantitative. The optimal mechanical activation time is 20min when it is substituted into the charging energy formula (I) for calculation.

[0079] Verify the validity of the formula

[0080] A mechanically activated starch inhibitor was prepared according to the optimal mechanical activation parameter set determined in step S4, and the starch activation inhibitor was subjected to a flotation experiment. The flotation recovery rate was 1%, and the starch inhibitor had the best effect, indicating that the method had high accuracy. The parameter combination in the above-mentioned optimal fitting group was the combination of the optimal mechanical activation parameter set.

[0081] Example 2

[0082] An activation method for optimizing mechanically activated starch inhibitors comprises the following steps:

[0083] S1. Preparation of mechanically activated starch inhibitor and calculation of charging energy

[0084] Weigh 4 g corn starch (NS) and place it in a planetary mill zirconia tank for later use;

[0085] The starch raw materials were dry-mechanically activated according to the planetary mill parameters set in experimental groups 6-11: the planetary mill speed was used as a variable, and the corn starch (NS) was mechanically activated for 20 min at 200 r / min, 300 r / min, 350 r / min, 450 r / min, 500 r / min, and 600 r / min under the conditions of ball milling time of 20 min at room temperature. The grinding ball and corn starch (NS) ball material ratio was 15:1. After the mechanical ball milling process was completed, the corresponding charging energy value was calculated according to the charging energy formula (I):

[0086]

[0087] Among them, E is the charging energy, f is the starch activation index, τ is the ball-to-material ratio, e iis the unit energy consumption of the planetary mill, N is the rotation speed of the planetary mill, T is the activation time, f, e i is a constant, f is the activation index of corn starch (NS), which is 1.26, and e i is the unit energy consumption of the planetary mill, which is 1.2 J / c. According to the different ball-to-material ratios, activation time, and planetary mill speeds set in the experimental groups 6-11, different ordinary corn activated starch inhibitors were obtained, and the charging energies were calculated to be 5.376 KJ, 8.064 KJ, 10.752 KJ, 13.440 KJ, and 16.128 KJ of mechanically activated corn starch (NS), respectively. In this embodiment, the inner diameter of the zirconia tank is 4 cm and the volume is 50 ml; the diameter of the grinding balls in the zirconia tank is 1 cm, and the grinding ball material is zirconia.

[0088] S2. Flotation test, record experimental data

[0089] The different common corn activated starch inhibitors obtained in step S1 are subjected to a mineral flotation experiment and a recovery test is performed to obtain a recovery rate ε. The flotation experiment steps are as follows:

[0090] Weigh 0.08g starch and use deionized water as solvent to prepare a 0.8g / L starch inhibitor solution; use the starch inhibitor solution as an inhibitor to perform flotation separation on different minerals, including the following steps (taking hematite flotation as an example): add 2g hematite (200-400 mesh) into a flotation tank, add 25ml deionized water and stir for 2min to form a slurry, adjust the pH of the slurry to 10, stir for 2min, add an aqueous solution (2ml) of a mechanically activated starch inhibitor to make the starch inhibitor concentration in the flotation tank 40mg / L, stir for 2min, then add 1mL 1.6g / L dodecylamine collector, stir for 2min, then add 2 drops of a frother, scrape the flotation foam, filter, dry and weigh the minerals in the tank, record the weighing data, and the recovery rate is the mass ratio of the concentrate mass in the tank to the mass of the weighed ore sample to be floated, and the corresponding flotation recovery rate is calculated, and the results are as follows: Figure 2 shown.

[0091] S3. SPSS fits the recovery rate and charging data to obtain the recovery rate-charging formula

[0092] The parameters in step S1, the charging energy (E) calculated under different parameter conditions, and the flotation recovery rate (ε) recorded in step S2 are sorted out to obtain Table 2:

[0093] Table 2 Parameters of corn starch (NS) inhibitor

[0094] category τ N(r / min) T(min) E(J) ε(%) Experimental Group 1 15 200 20 5376 18 Experimental Group 2 15 300 20 8064 9 Experimental Group 3 15 350 20 9408 8 Experimental Group 4 15 450 20 12096 10 Experimental Group 5 15 500 20 13440 16 Experimental Group 6 15 600 20 16128 22 Fitting the best group 15 400 20 10752 1

[0095] The charging energy (E) and flotation recovery (ε) in the above data were fitted by SPSS, and the results are as follows Figure 4 As shown in the figure, the fitting relationship between the inhibition recovery rate and the charging energy of ordinary corn activated starch is: ε=0.002E 2 -0.043E+0.24, which is the recovery rate-charging formula of ordinary corn starch, and the goodness of fit R 2 =0.98, goodness of fit R 2 ≥0.9.

[0096] S4. Determine the optimal charging energy value E i and the optimal mechanical activation parameter set

[0097] By taking the derivative and taking the extreme value through the recovery rate-charging formula, the optimal charging energy value is 10750KJ. In this embodiment, only the planetary mill speed is a variable, and the ball-to-material ratio and activation time are quantitative. The optimal planetary ball mill speed is 400r / min when it is substituted into the charging energy formula (I) for calculation.

[0098] S5. Prepare a mechanically activated starch inhibitor based on the optimal mechanical activation parameter set.

[0099] Verify the validity of the formula

[0100] According to the optimal mechanical activation parameter set determined in step S4, a mechanically activated starch inhibitor was prepared, and the starch activation inhibitor was subjected to a flotation experiment. The flotation recovery rate was 1%, and the starch inhibitor had the best effect, indicating that the accuracy of the method was high. The parameter combination in the above-mentioned optimal fitting group 1 was the combination of the optimal mechanical activation parameter set.

[0101] Example 3

[0102] An activation method for optimizing mechanically activated starch inhibitors comprises the following steps:

[0103] S1. Preparation of mechanically activated starch inhibitor and calculation of charging energy

[0104] Weigh 4 g corn starch (NS) and place it in a planetary mill zirconia tank for later use;

[0105] The starch raw materials were dry-mechanically activated according to the planetary mill parameters set in experimental groups 12-15: with the ball-to-material ratio as a variable, corn starch (NS) was mechanically activated for 20 min at room temperature using a planetary mill at a speed of 400 r / min. The grinding ball and corn starch (NS) ball-to-material ratios were 10:1, 20:1, and 30:1. After the mechanical ball milling process was completed, the corresponding charging energy value was calculated according to the charging energy formula (I):

[0106]

[0107] Among them, E is the charging energy, f is the starch activation index, τ is the ball-to-material ratio, ei is the unit energy consumption of the planetary mill, N is the rotation speed of the planetary mill, T is the activation time, f, e i is a constant, f is the activation index of corn starch (NS), which is 1.26, and e i is the unit energy consumption of the planetary mill, which is 1.2 J / c. According to the different ball-to-material ratios, activation time, and planetary mill speeds set in the experimental groups 12-15, different ordinary corn activated starch inhibitors were obtained, and the charging energies were calculated to be 10.842 KJ, 10.584 KJ, and 10.416 KJ of mechanically activated corn starch (NS), respectively. In this embodiment, the inner diameter of the zirconia tank is 4 cm and the volume is 50 ml; the diameter of the grinding balls in the zirconia tank is 1 cm, and the grinding ball material is zirconia.

[0108] S2. Flotation test, record experimental data

[0109] The different common corn activated starch inhibitors obtained in step S1 are subjected to a mineral flotation experiment and a recovery test is performed to obtain a recovery rate ε. The flotation experiment steps are as follows:

[0110] Weigh 0.08g starch and use deionized water as solvent to prepare a 0.8g / L starch inhibitor solution; use the starch inhibitor solution as an inhibitor to perform flotation separation on different minerals, including the following steps (taking hematite flotation as an example): add 2g hematite (200-400 mesh) into a flotation tank, add 25ml deionized water and stir for 2min to form a slurry, adjust the pH of the slurry to 10, stir for 2min, add an aqueous solution (2ml) of a mechanically activated starch inhibitor to make the starch inhibitor concentration in the flotation tank 40mg / L, stir for 2min, then add 1mL 1.6g / L dodecylamine collector, stir for 2min, then add 2 drops of a frother, scrape the flotation foam, filter, dry and weigh the minerals in the tank, record the weighing data, and the recovery rate is the mass ratio of the concentrate mass in the tank to the mass of the weighed ore sample to be floated, and the corresponding flotation recovery rate is calculated, and the results are as follows: Figure 3 shown.

[0111] S3. SPSS fits the recovery rate and charging data to obtain the recovery rate-charging formula

[0112] The parameters in step S1, the charging energy (E) calculated under different parameter conditions, and the flotation recovery rate (ε) recorded in step S2 are sorted out to obtain Table 3:

[0113] Table 3 Parameters of corn starch (NS) inhibitor

[0114] category τ N(r / min) T(min) E(J) ε(%) Experimental Group 1 10 200 20 10842 18 Experimental Group 2 20 300 20 10584 9 Experimental Group 3 30 350 20 10416 16 Fitting the best group 15 400 20 10752 1

[0115] The charging energy (E) and flotation recovery (ε) in the above data were fitted by SPSS, and the results are as follows Figure 4 As shown in the figure, the fitting relationship between the inhibition recovery rate and the charging energy of ordinary corn activated starch is: ε=0.002E 2 -0.043E+0.24, which is the recovery rate-charging formula of ordinary corn starch, and the goodness of fit R 2 =0.98, goodness of fit R 2 ≥0.9.

[0116] S4. Determine the optimal charging energy value E i and the optimal mechanical activation parameter set

[0117] By taking the derivative of the recovery rate-charging energy formula and taking the extreme value, the optimal charging energy value is 10750KJ. In this embodiment, only the ball-to-material ratio is a variable, and the activation time and the planetary mill speed are quantitative. The optimal ball-to-material ratio is 15:1 when it is substituted into the charging energy formula (I) for calculation.

[0118] In summary, according to Examples 1-3, the best mechanical activation conditions are: mechanical activation time 20 min, planetary ball mill speed 400 r / min, ball-to-material ratio 15:1.

[0119] S5. Prepare a mechanically activated starch inhibitor based on the optimal mechanical activation parameter set.

[0120] Verify the validity of the formula

[0121] A mechanically activated starch inhibitor was prepared according to the optimal mechanical activation parameter set determined in step S4, and the starch activation inhibitor was subjected to a flotation experiment. The flotation recovery rate was 1%, and the starch inhibitor had the best effect, indicating that the method had high accuracy. The parameter combination in the above-mentioned optimal fitting group was the combination of the optimal mechanical activation parameter set.

[0122] Embodiment 4-6

[0123] By changing the starch raw materials to WS, G50, and G80 and repeating the above steps, the optimal mechanical activation time for WS was 10 min, the optimal planetary ball mill speed was 400 r / min, and the optimal ball-to-material ratio was 15:1; the optimal mechanical activation time for G50 was 20 min, the optimal planetary ball mill speed was 500 r / min, and the optimal ball-to-material ratio was 15:1; the optimal mechanical activation time for G80 was 30 min, the optimal planetary ball mill speed was 400 r / min, and the optimal ball-to-material ratio was 15:1.

[0124] In the present application, NS, WS, G50 and G80 are mechanically activated by planetary ball milling for a relatively short period of time, so that the chemical reaction activity of the activated NST, WST, G50T and G80T is improved, and the chemical adsorption capacity with minerals during flotation is improved, so that the minerals are made hydrophilic and the combination of the minerals and the collector is hindered. The mechanically activated starch acts as an inhibitor, which greatly reduces the flotation recovery rate.

[0125] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. An activation method for optimizing mechanically activated starch inhibitors, characterized in that: The following steps are involved: S1. Using starch as raw material, adjusting the mechanical activation parameter set of the planetary mill, performing dry mechanical activation solid phase reaction to charge the starch raw material, obtaining mechanically activated starch inhibitors under different parameter conditions, and calculating the charging energy value of each mechanically activated starch inhibitor; S2. Using the mechanically activated starch as an inhibitor, flotation experiments were performed on the minerals, and the flotation recovery rates were recorded; S3. Use SPSS to fit the corresponding charging energy value and flotation recovery rate to obtain the recovery rate-charging formula (Ⅱ), (Ⅱ), Where ε is the flotation recovery rate; α, β, and γ are constants determined by the type of starch; S4. Calculate the optimal charging energy value E through the recovery rate-charging formula (Ⅱ) i , E i Substitute it into the charging energy formula (I) to reversely determine the optimal mechanical activation parameter set; Optimal charging energy value E i The calculation method is to take the derivative of the recovery rate-charging formula (II) equal to zero, and the extreme value is the optimal charging energy value E i , E i The process of inversely determining the optimal mechanical activation parameter set by inserting the charging energy value E into the charging energy formula (I) is as follows: i Substitute into the charging energy formula (I), calculate the remaining parameter based on any two parameters in the mechanical activation parameter set, and record the obtained three parameters as the optimal mechanical activation parameter set, wherein the mechanical activation parameter set includes three parameters: ball-to-material ratio, planetary mill speed, and activation time; S5. Preparing a mechanically activated starch inhibitor based on the optimal set of mechanical activation parameters; The charging energy value is calculated by the charging energy formula (I). (Ⅰ), Among them, E is the charging energy, f is the starch activation index, τ is the ball-to-material ratio, e i is the unit energy consumption of the planetary mill, N is the rotation speed of the planetary mill, and T is the activation time.

2. The method for activating the optimized mechanically activated starch inhibitor according to claim 1, characterized in that: The starch raw material includes one or more of corn starch, potato starch, glutinous rice starch and rice starch.

3. The method for activating the optimized mechanically activated starch inhibitor according to claim 1, characterized in that: In step S1, the charging energy value ranges from 2.6KJ to 32KJ.

4. The method for activating the optimized mechanically activated starch inhibitor according to claim 1, characterized in that: The flotation experiment comprises the following steps: adding deionized water to the ore sample to be floated, adjusting the pH to alkaline, adding the aqueous solution of the mechanically activated starch inhibitor, stirring, adding a collector, stirring, flotation and scraping bubbles, filtering the product in the tank, drying and weighing, and obtaining the grade and recovery rate of the flotation concentrate.