Catalyst compound, preparation method, olefin polymerization catalyst and application

By using a single titanocene compound with a condensed heterobicycloheptane structure and a cocatalyst, a catalytic system is formed, which solves the problems of poor polymer molecular weight and molecular distribution in the existing technology, and achieves efficient preparation of polymers with high molecular weight and narrow molecular weight distribution. things.

CN115651011BInactive Publication Date: 2024-10-22QINGDAO XUANDAO TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211098017.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-08
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing technology is difficult to prepare polymers with high molecular weight and narrow molecular weight distribution in olefin polymerization, and the structure of the catalyst has little effect on the polymerization performance, making it difficult to effectively suppress the chain transfer reaction.

Method used

A single titanocene compound with a condensed heterobicycloheptane structure is used as a catalyst, Compound B and Compound C are used to prepare the catalyst through a specific synthesis method, and alkylaluminoxane and an organic boron compound are used as cocatalysts to form a catalytic system for catalysis Ethylene homopolymerization and ethylene/α-olefin/cyclic olefin copolymerization.

Benefits of technology

The catalytic activity and thermal stability are improved, and the chain transfer reaction is suppressed. The obtained polymer has a high molecular weight and a narrow molecular weight distribution, and is suitable for the efficient preparation of polyethylene, polyolefin elastomers and cyclic olefin copolymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003839171330000021
    Figure BDA0003839171330000021
  • Figure BDA0003839171330000041
    Figure BDA0003839171330000041
  • Figure BDA0003839171330000052
    Figure BDA0003839171330000052
Patent Text Reader

Abstract

The present invention relates to a kind of catalyst compound, preparation method, olefin polymerization catalyst and application, wherein the catalyst compound is for olefin polymerization catalyst, containing thick bicycloheptane structure, the introduction of bicycloheptane improves the spatial effect and charge property of transition metal, is conducive to stabilizing metal cation center, makes it have the characteristics of high catalytic activity, good thermal stability, high comonomer insertion rate, contrast common aryloxy or arylthio, bicycloheptane structure electron-donating ligand has larger steric hindrance, can effectively suppress the chain transfer reaction in polymerization, so as to obtain a polymer with higher molecular weight. The catalyst using the catalyst compound is suitable for ethylene and alpha-olefin homopolymerization, ethylene and alpha-olefin / cycloolefin copolymerization, and polyolefin materials such as polyethylene, polyolefin elastomer, and cycloolefin copolymer can be efficiently prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of olefin polymerization, and in particular relates to a catalyst for olefin polymerization, and specifically relates to a catalyst compound, a preparation method, an olefin polymerization catalyst and application. Background Art

[0002] Materials are one of the important material foundations for social development, among which polymer materials are playing an increasingly important role due to their outstanding performance. Among all polymer materials, polyolefin materials are the fastest growing and largest-yielding synthetic resins, and have become an important pillar of modern society and scientific and technological development. They are widely used in various fields of industrial production and daily life due to their excellent compatibility, processability, weather resistance and other excellent properties. In recent years, high-end polyolefin materials such as polyolefin elastomers (POE), cycloolefin copolymers (COC), olefin block copolymers (OBC) have gradually been developed and applied. In olefin polymerization reactions, catalysts determine olefin polymerization behavior, polymer structure and performance, and are the core of polyolefin development.

[0003] Compared with traditional Ziegler-Natta catalysts, metallocene catalysts have a single catalytic active center and can produce polyolefin products with uniform relative molecular weight, structure and composition. At the same time, the parameters of the polymer can be controlled by the structure of the catalyst, such as relative molecular weight and distribution, polymer regularity, content and distribution of comonomers, etc. In recent years, single metallocene catalysts with electron-donating ligands have received increasing attention. This type of catalyst shows high catalytic activity in olefin polymerization, and exhibits good comonomer insertion ability in ethylene homopolymerization and copolymerization of ethylene with α-olefins / styrene / cycloolefins, etc., while ensuring high polymerization activity, polymers with high molecular weight and high comonomer content are obtained. Patent US 5064802, 1991 reported that the catalytic system composed of compound a and triethylammonium tetrakis(pentafluorophenyl)borate catalyzed ethylene (1atm) polymerization at room temperature with a polymerization activity of 1.23×10 4 g polymer / (mol Tih); Serrano et al. established a synthesis method for compound b (see Journal of organometallic chemistry, 1991, 419 (1-2): 77-84.). Thereafter, Nomura et al. reported the study of a single metallocene Cp′Ti(Oar)Cl2 (compound be) with an aromatic radical as a catalyst for olefin polymerization, including homopolymerization of ethylene and α-olefins, copolymerization of ethylene with α-olefins / cycloolefins, etc. The polymerization activity was closely related to the catalyst structure, and the substituents on the Cp′ ligand and the aromatic radical strongly affected the polymerization behavior (see Organometallics, 1998, 17 (11): 2152-2154; Macromolecules, 2000, 33 (9): 3187-3189; Macromolecules, 2003, 36 (11): 3797-3799). For example, in the process of catalyzing the copolymerization of ethylene and norbornene, compound e exhibited significant catalytic activity and high NB monomer insertion rate, synthesizing a high molecular weight polymer with a unimodal molecular weight distribution; the copolymerization activity of compound b was relatively low, which decreased with the increase of the initial concentration of NB monomer, and showed less NB monomer insertion rate compared with compound e under the same conditions; compound c showed a better NB monomer insertion rate than b, but its catalytic activity was lower than that of b and e.

[0004]

[0005] In the research of catalysts, polyolefins with different molecular weights, isotacticity, comonomer insertion rates, etc. can be obtained by modifying the catalyst auxiliary ligands, so the structure of the catalyst has a very obvious effect on the olefin polymerization performance. Although such metallocene catalysts are already available in the prior art, researching and developing new ligands to prepare new monometallic transition metal catalysts is still an important topic for the preparation of olefin polymers. Summary of the invention

[0006] The object of the present invention is to provide a catalyst compound, a preparation method, an olefin polymerization catalyst and application, so as to further improve the olefin polymerization performance in the background technology.

[0007] To achieve the above technical objectives, this application is implemented through the following technical solutions:

[0008] A catalyst compound, the structural formula of the compound is shown in Formula I:

[0009] In formula I, M is one or more of transition metal atoms of Groups IVB, VB, VIIB, and VIII; and / or Cp' is a cyclopentadienyl, indenyl, or fluorenyl group which is substituted or unsubstituted with a hydrocarbon group; and / or X1 and X2 are each independently selected from an alkyl group, an aryl group, an alkoxy group, an aryloxy group, or a halogen atom; and / or R1 is an oxygen atom, a sulfur atom, an alkyl group, or an alkoxy group; and / or R2 is a hydrogen atom, an alkyl group, an aryl group, a substituted alkyl group, or a substituted aryl group.

[0010] Preferably, in formula I, M is preferably a transition metal atom of Group IVB and / or VB; Cp' is a C1-C12 alkyl group, a C6-C12 aryl group, a trimethylsilyl-substituted or unsubstituted cyclopentadienyl group, an indenyl group or a fluorenyl group; X1 and X2 are each independently selected from a C1-C5 alkoxy group, a C6-C9 aryloxy group, a C1-C5 alkyl group, a C6-C9 aryl group or a halogen atom; R1 is an oxygen atom, a sulfur atom, a C1-C3 alkyl group or an alkoxy group; R2 is a hydrogen atom, a C1-C6 alkyl group, an aryl group, a substituted alkyl group or a substituted aryl group.

[0011] Preferably, in formula I, M is preferably titanium, zirconium, hafnium, and is further preferably selected from titanium or zirconium; Cp' is selected from cyclopentadienyl, pentamethylcyclopentadienyl, indenyl, or fluorenyl, and is further preferably selected from cyclopentadienyl, pentamethylcyclopentadienyl or indenyl; X1 and X2 are each independently selected from methyl, phenyl, benzyl, methoxy, phenoxy or chlorine atom, and are further preferably selected from chlorine atom or methyl; R1 is selected from oxygen atom, sulfur atom, methylene, ethylene or methyleneoxy, and is further preferably selected from oxygen atom or methyleneoxy; R2 is selected from hydrogen atom, methyl, ethyl, cyclohexyl, phenyl or substituted phenyl, and is further preferably selected from hydrogen atom.

[0012] Preferably, the catalyst compound of the present invention is shown in the following (1)-(8):

[0013]

[0014] The catalyst compound is prepared from compound B and compound C, wherein the structural formula of compound B is shown in formula II, and the structural formula of compound C is shown in formula III, wherein formula II is Formula III is Wherein formula III contains a fused bicycloheptane structure;

[0015] In formula II, M is preferably titanium, zirconium, hafnium, and is further preferably selected from titanium or zirconium; Cp' is selected from cyclopentadienyl, pentamethylcyclopentadienyl, indenyl, or fluorenyl, and is further preferably selected from cyclopentadienyl, pentamethylcyclopentadienyl, or indenyl; X is selected from methyl, phenyl, benzyl, methoxy, phenoxy, and chlorine atom, and is further preferably selected from chlorine atom or methyl.

[0016] In formula (III), R3 is selected from hydroxyl, hydroxymethyl, hydroxyethyl, mercapto, chlorine, bromine, iodine, chloromethyl, bromomethyl or iodomethyl, preferably hydroxyl or hydroxymethyl; R2 is selected from hydrogen, methyl, ethyl, cyclohexyl, phenyl or substituted phenyl, preferably hydrogen. It should be noted that R3 can be substituted at the 1-position, 2-position or 7-position of bicycloheptane.

[0017] In the present invention, the compound C of formula III can be prepared from the compound D of formula IV as the main raw material according to the method disclosed in the prior art (e.g. Journal of the American Chemical Society, 1994, 116 (6): 2424-2429). Of course, other methods for preparing the compound C of formula III using the compound of formula IV can also be applied. Formula IV is as follows:

[0018] Wherein, the compound D shown in formula IV includes those shown in formula (IV-1) to formula (IV-7) (the synthesis method thereof can be found in Journal of Molecular Catalysis A: Chemical, 2004, 213(1):81-87).

[0019]

[0020] In addition, the compound D shown in formula IV can be a cyclonorbornene, including (IV-8) to (IV-13) in addition to the monosubstituted norbornene shown in formula (IV-1) to (IV-7) (the synthesis method thereof can be seen in Macromolecular Chemistry and Physics, 2016, 217 (24): 2708-2716).

[0021]

[0022] A method for preparing any of the above catalyst compounds, carried out under a protective atmosphere, comprises the following steps:

[0023] S1, mixing the compound B represented by formula II with a solvent to obtain a solution D;

[0024] S2, mixing the compound C represented by formula III, a solvent and a set amount of alkyl lithium, and reacting to obtain a solution E;

[0025] S3. Add solution E dropwise into solution D to obtain a catalyst compound through reaction.

[0026] The protective atmosphere is nitrogen or argon.

[0027] The solvent is an organic solvent, including tetrahydrofuran, dichloromethane, toluene, diethyl ether, etc., preferably diethyl ether or toluene; and / or in step (1) and step (2), the molar ratio of the compound represented by formula (II) to that represented by formula (III) is 1:(2-1), preferably 1:(1.2:1); and / or in step (2), the alkyl lithium includes but is not limited to methyl lithium, ethyl lithium, propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, preferably n-butyl lithium; the molar ratio of the alkyl lithium to the compound represented by formula (III) is greater than 1:1, preferably (1.2-5):1.

[0028] In step (2), the reaction is carried out at -100°C-0°C, preferably at -78°C--20°C, and more preferably at -78°C; in step (2), the reaction is carried out for 12-48 hours, preferably 18-24 hours; in step (3), the reaction is carried out at -100°C-0°C, preferably at -78°C--20°C, and more preferably at -78°C; in step (3), the reaction is carried out for 12-48 hours, preferably 18-24 hours; after the reaction in step (3), post-treatment is carried out, and the post-treatment sequentially includes solvent removal, extraction and freeze crystallization.

[0029] The post-treatment is carried out as follows: vacuum removal of the solvent, toluene extraction, filtration with diatomaceous earth filter aid, and freezing and crystallization of the filtrate at below -10°C (preferably below -25°C). After crystallization, the mother liquor is removed, and the remaining solid is vacuum dried to obtain a catalyst compound.

[0030] A catalyst for olefin polymerization using any one of the above-mentioned catalyst compounds as a catalyst.

[0031] It also includes alkylaluminoxane and / or alkylaluminum and organic boron compound composition as a co-catalyst and a catalyst compound to form a catalyst system.

[0032] The alkylaluminoxane includes but is not limited to methylaluminoxane, ethylaluminoxane, isobutylaluminoxane and alkyl-modified methylaluminoxane, preferably methylaluminoxane and alkyl-modified methylaluminoxane; the alkylaluminum includes but is not limited to trimethylaluminum, triethylaluminum, triisobutylaluminum, preferably triisobutylaluminum; the boron compound co-catalyst includes but is not limited to tris(pentafluorophenyl)borane, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate and N,N-dimethylbenzylammonium tetrakis(pentafluorophenyl)borate; preferably tris(pentafluorophenyl)borane and triphenylcarbon tetrakis(pentafluorophenyl)borate.

[0033] The molar ratio of the catalyst compound to the alkylaluminoxane is 1:50-20000, preferably 1:(500-5000), wherein the molar amounts of the M element and aluminum are used respectively; the molar ratio of the catalyst compound to the alkylaluminum and organic boron compound composition is 1:50-20000:1-3, preferably 1:(1-1.5):(50-200), wherein the molar amounts of the M element, aluminum element and boron element are used respectively.

[0034] An application of an olefin polymerization catalyst, any of the above olefin polymerization catalysts, for catalyzing ethylene homopolymerization and / or ethylene and α-olefin / cycloolefin copolymerization. The reaction also includes an organic solvent, preferably toluene, xylene, cyclohexane, more preferably toluene. The reaction temperature is -50°C to 250°C, more preferably 25°C to 150°C.

[0035] The beneficial effects of the present invention are:

[0036] The catalyst compound used for the catalyst for olefin polymerization of the present invention contains a condensed bicycloheptane structure. The introduction of bicycloheptane improves the spatial effect and charge properties of the transition metal, is conducive to stabilizing the metal cation center, and has the characteristics of high catalytic activity, good thermal stability, and high comonomer insertion rate. Compared with ordinary aryloxy or arylthio groups, the electron-donating ligand of the bicycloheptane structure has greater steric hindrance, which can effectively inhibit the chain transfer reaction in the polymerization, thereby obtaining a polymer with a higher molecular weight. Therefore, the catalyst is suitable for homopolymerization of ethylene and alpha-olefin, copolymerization of ethylene and alpha-olefin / cycloolefin, and can efficiently prepare polyolefin materials such as polyethylene, polyolefin elastomer, and cycloolefin copolymer.

[0037] The polymerization system of the present invention adopts a mono-titanocene compound with a special bicycloheptane structure, and the preparation process is simple, safe and efficient. At the same time, the obtained polymer has the advantages of high molecular weight, narrow molecular weight distribution and the like. DETAILED DESCRIPTION

[0038] Compared with the existing aryloxy or arylthio groups, the catalyst compound used in the olefin polymerization catalyst of the present invention has a condensed bicycloheptane structure, which further improves the spatial effect and charge properties of the transition metal, is beneficial to stabilizing the metal cation center, and has the characteristics of high catalytic activity, good thermal stability, and high comonomer insertion rate. The electron-donating ligand of the bicycloheptane structure has greater steric hindrance, which can effectively inhibit the chain transfer reaction in the polymerization, thereby obtaining a polymer with a higher molecular weight.

[0039] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0040] In addition, the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0041] The raw materials of the examples and comparative examples of the present invention can be obtained from the market or prepared by the methods disclosed in the prior art, and the solvents and monomers therein are treated to be anhydrous and oxygen-free.

[0042] Example 1 Synthesis of Catalyst Compound A1:

[0043] Step 1: Place a dry magnet in a 250 mL Shrek bottle, place the reaction bottle in a magnetic stirring device, and then perform three vacuum-filling and nitrogen-filling operations to replace the air in the bottle, allowing the reaction to proceed under an inert atmosphere. At -78 ° C, slowly add a n-BuLi (10 mL / 25 mmol, 2.5 M) n-hexane solution to a frozen diethyl ether solution of bicyclo[2.2.1]heptane-2-ol (2.24 g / 20 mmol). Then warm to room temperature and react overnight to obtain (C7H 11 O)Li salt solution. The solution was distilled under reduced pressure to remove the solvent and obtain a light yellow (C7H 11 O) Li salt solid 2.1 g / 17.8 mmol, yield about 89.0%.

[0044] Step 2: Use toluene to obtain (C7H 11 O)Li salt solid dissolved, at -78 ° C conditions, (C7H 11 The toluene solution of CpTiCl3 (3.9 g / 17.8 mmol) was slowly added to the toluene solution of Li (2.1 g / 17.8 mmol), and then the temperature was raised to room temperature and the reaction was allowed to proceed overnight. The solution was filtered through a diatomaceous earth filter aid to remove LiCl, the solvent was removed in vacuo at room temperature, and the mixture was extracted with dry toluene, followed by freezing and crystallization at -25°C. After filtering the solvent, the remaining crystals were dried under reduced pressure to obtain 3.99 g / 13.5 mmol of a dark red (cyclopentadienyl) (dicycloheptyl-2-oxy) titanium dichloride solid, with a yield of about 75.84%.

[0045] 1H-NMR (CDCl3, 25°C): δ = 6.5 (Cp*, 4H), 2.9 (2H), 1.4-1.55 (10H), 3.16 (1H).

[0046] Example 2 Synthesis of Catalyst Compound A2:

[0047] Step 1: Same as Example 1, obtain light yellow (C7H 11 O) Li salt solid 1.9 g / 16.1 mmol, yield about 80.5%.

[0048] Step 2: Similar to Example 1, CpTiCl3 is replaced with Me5CpTiCl3 to obtain 4.32 g / 11.8 mmol of reddish brown (pentamethylcyclopentadienyl)(dicycloheptyl-2-oxy) titanium dichloride solid with a yield of about 73.29%.

[0049] 1 H-NMR (CDCl3, 25°C): δ = 1.71 (Cp*, 12H), 1.26 (3H), 3.07 (1H), 1.4-1.55 (10H), 3.16 (1H).

[0050] Example 3 Synthesis of Catalyst Compound A5:

[0051] Step 1: Place a dry magnet in a 250 ml Shrek bottle, place the reaction bottle in a magnetic stirring device, and then perform three vacuum-filling and nitrogen-filling operations to replace the air in the bottle and allow the reaction to proceed under an inert atmosphere. At -78°C, slowly add a n-BuLi (10 mL / 25 mmol, 2.5 M) hexane solution to a frozen 2-(hydroxymethyl)bicyclo[2.2.1]heptane (2.52 g / 20 mmol) ether solution. Then warm to room temperature and react overnight to obtain (C8H 14 O)Li salt solution. The solution was distilled under reduced pressure to remove the solvent and obtain a yellow (C8H 14 O) Li salt solid 2.19 g / 16.59 mmol, yield about 82.95%.

[0052] Step 2: Similar to Example 1, (C7H 11 O)Li is replaced by (C8H 14 O)Li, and 4.1 g / 13.22 mmol of black-red (cyclopentadienyl)(dicycloheptyl-2-methyleneoxy)titanium dichloride solid was obtained, with a yield of about 79.68%.

[0053] 1H-NMR (CDCl3, 25°C): δ = 6.4-6.5 (Cp*, 4H), 2.9 (2H), 1.36-1.51 (11H), 3.49 (2H).

[0054] Example 4 Synthesis of Catalyst Compound A6:

[0055] Step 1: Same as Example 3, obtain yellow (C8H 14 O) Li salt solid 2.3 g / 17.42 mmol, yield about 87.1%.

[0056] Step 2: Similar to Example 3, CpTiCl3 is replaced with Me5CpTiCl3 to obtain (pentamethylcyclopentadienyl)(dicycloheptyl-2-methyleneoxy)titanium dichloride solid 5.48 g / 15.05 mmol, with a yield of about 86.39%.

[0057] 1 H-NMR (CDCl3, 25°C): δ = 1.71 (Cp*, 12H), 1.26 (3H), 3.07 (1H), 1.36-1.51 (11H), 3.49 (2H).

[0058] Example 5 Synthesis of Catalyst Compound A3:

[0059] Step 1: Same as Example 1, obtain light yellow (C7H 11 O) Li salt solid 2.07 g / 17.54 mmol, yield about 87.7%.

[0060] Step 2: Similar to Example 1, CpTiCl3 is replaced with IndTiCl3 to obtain brown-red (indenyl)(dicycloheptyl-2-oxy) titanium dichloride solid 4.1 g / 11.85 mmol, with a yield of about 67.56%.

[0061] 1 H-NMR (CDCl3, 25°C): δ=3.22(2H), 6.39(1H), 6.58(1H), 7.0-7.2(4H), 3.16(1H), 1.40-1.55(10H).

[0062] Example 6 Synthesis of Catalyst Compound A7:

[0063] Step 1: Same as Example 1, obtain light yellow (C7H 11 O) Li salt solid 1.73 g / 14.66 mmol, yield about 73.3%.

[0064] Step 2: Similar to Example 1, CpTiCl3 is replaced with CpZrCl3 to obtain 4.11 g / 12.12 mmol of purple-black (cyclopentadienyl)(dicycloheptyl-2-oxy) zirconium dichloride solid with a yield of about 82.67%.

[0065] 1 H-NMR (CDCl3, 25°C): δ = 6.5 (Cp*, 4H), 2.9 (2H), 1.4-1.55 (10H), 3.16 (1H).

[0066] Example 7 Synthesis of Catalyst Compound A8:

[0067] Step 1: Same as Example 1, obtain light yellow (C7H 11 O) Li salt solid 2.13 g / 18.05 mmol, yield about 90.25%.

[0068] Step 2: Similar to Example 1, CpTiCl3 is replaced with MeCpZrCl3 to obtain 5.69 g / 13.91 mmol of purple (pentamethylcyclopentadienyl) (dicycloheptyl-2-oxy) zirconium dichloride solid with a yield of about 77.06%.

[0069] 1 H-NMR (CDCl3, 25°C): δ = 1.71 (Cp*, 12H), 1.26 (3H), 3.07 (1H), 1.4-1.55 (10H), 3.16 (1H).

[0070] Example 8 Synthesis of Catalyst Compound A4:

[0071] The compound (cyclopentadienyl) (dicycloheptyl-2-oxy) titanium dichloride (1.5 g / 5.07 mmol) was dissolved in 100 mL of ether. At -40 ° C, a solution of MeLi (6.8 mL / 10.88 mmol, 1.6 M) in ether was slowly added to the frozen solution of (cyclopentadienyl) (dicycloheptyl-2-oxy) titanium dichloride in ether, then warmed to room temperature and reacted overnight. The solution was desolventized and the residue was extracted with n-hexane. An ether solution of MeMgBr (2 mL / 6 mmol, 3 M) was added to the n-hexane solution, and the resulting mixture was stirred at room temperature for 2 h. The solvent was then removed and the residue was extracted with n-hexane. The n-hexane solution was concentrated and frozen (-25 ° C) overnight to obtain orange-yellow (cyclopentadienyl) (dicycloheptyl-2-oxy) dimethyl titanium 0.79 g / 3.1 mmol, with a yield of about 61.14%.

[0072] 1H-NMR (CDCl3, 25°C): δ = 6.5 (Cp*, 4H), 2.9 (2H), 1.4-1.55 (10H), 3.16 (1H), 0.9 (6H).

[0073] Example 9 Catalyst Compound A1 is used as a catalyst to catalyze ethylene polymerization:

[0074] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A1 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 5.82×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 3.24 × 10 5 g / mol.

[0075] Example 10 Catalyst Compound A2 is used as a catalyst to catalyze ethylene polymerization:

[0076] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A2 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 3.34×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 2.16 × 10 5 g / mol.

[0077] Example 11 Catalyst Compound A3 is used as a catalyst to catalyze ethylene polymerization:

[0078] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A3 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 6.73×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 4.5 × 10 5 g / mol.

[0079] Example 12 Catalyst Compound A4 is used as a catalyst to catalyze ethylene polymerization:

[0080] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A4 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 8.79×10 5 g polymer / (mol Ti h), polymer molecular weight Mw = 2.67 × 10 5 g / mol.

[0081] Example 13 Catalyst Compound A5 is used as a catalyst to catalyze ethylene polymerization:

[0082] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly pumped and filled with nitrogen for several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of alkyl-modified methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A5 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 3.28×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 2.2 × 10 5 g / mol.

[0083] Example 14 Catalyst Compound A6 is used as a catalyst to catalyze ethylene polymerization:

[0084] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of alkyl-modified methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A6 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 1.74×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 2.01 × 10 5 g / mol.

[0085] Example 15 Catalyst Compound A7 is used as a catalyst to catalyze ethylene polymerization:

[0086] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A7 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 6.1×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 4.47 × 10 5 g / mol.

[0087] Example 16 Catalyst Compound A8 is used as a catalyst to catalyze ethylene polymerization:

[0088] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of the catalyst compound A8 (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system was about 4.29×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 3.74 × 10 5 g / mol.

[0089] Example 17 Catalyst Compound A1 is used as a catalyst to catalyze ethylene / norbornene copolymerization:

[0090] The polymerization kettle was heated to 120°C, vacuumed and filled with nitrogen several times, and finally the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 80°C, 100mL of toluene solution of norbornene (6M) and 0.4mmol of triisobutylaluminum were added, and the liquid phase and gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of catalyst compound A1 (2μmol / L) and a toluene mixed solution of triphenylcarbon tetrakis (pentafluorophenyl) borate with a 1.1 times equivalent relative to Ti were added, and ethylene was introduced at a pressure of 10atm, the pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 6.06×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 5.21 × 10 5 The glass transition temperature Tg of the copolymer of ethylene and norbornene is 92.6°C.

[0091] Example 18 Catalyst Compound A2 is used as a catalyst to catalyze ethylene / norbornene copolymerization:

[0092] The polymerization kettle was heated to 120°C, vacuumed and filled with nitrogen several times, and finally replaced with ethylene, and cooled to room temperature. The temperature of the polymerization kettle was set to 80°C, 100mL of toluene solution of norbornene (6M) and 0.4mmol of triisobutylaluminum were added, and the liquid phase and gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of catalyst compound A2 (2μmol / L) and a toluene mixed solution of triphenylcarbon tetrakis (pentafluorophenyl) borate with a 1.1 times equivalent relative to Ti were added, and ethylene was introduced at a pressure of 10atm, and the pressure in the polymerization kettle was maintained at 5atm. The polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 3.7×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 2.53 × 10 5 The glass transition temperature Tg of the copolymer of ethylene and norbornene is 76°C.

[0093] Example 19 Catalyst Compound A3 is used as a catalyst to catalyze ethylene / norbornene copolymerization:

[0094] The polymerization kettle was heated to 120°C, vacuumed and filled with nitrogen several times, and finally replaced with ethylene, and cooled to room temperature. The temperature of the polymerization kettle was set to 80°C, 100mL of toluene solution of norbornene (6M) and 0.4mmol of triisobutylaluminum were added, and the liquid phase and gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of catalyst compound A3 (2μmol / L) and a toluene mixed solution of triphenylcarbon tetrakis (pentafluorophenyl) borate with a 1.1 times equivalent relative to Ti were added, and ethylene was introduced at a pressure of 10atm, and the pressure in the polymerization kettle was maintained at 5atm. The polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 7.37×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 5.9 × 10 5 The glass transition temperature Tg of the copolymer of ethylene and norbornene is 108.1°C.

[0095] Example 20 Catalyst Compound A5 is used as a catalyst to catalyze ethylene / norbornene copolymerization:

[0096] The polymerization kettle was heated to 120°C, vacuumed and filled with nitrogen several times, and finally replaced with ethylene, and cooled to room temperature. The temperature of the polymerization kettle was set to 80°C, 100mL of toluene solution of norbornene (6M) and 0.4mmol of triisobutylaluminum were added, and the liquid phase and gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of catalyst compound A5 (2μmol / L) and a toluene mixed solution of triphenylcarbon tetrakis (pentafluorophenyl) borate with a 1.1 times equivalent relative to Ti were added, and ethylene was introduced at a pressure of 10atm, and the pressure in the polymerization kettle was maintained at 5atm. The polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 1.74×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 2.09 × 10 5 The glass transition temperature Tg of the copolymer of ethylene and norbornene is 63°C.

[0097] Example 21 Catalyst Compound A7 is used as a catalyst to catalyze ethylene / norbornene copolymerization:

[0098] The polymerization kettle was heated to 120°C, vacuumed and filled with nitrogen several times, and finally replaced with ethylene, and cooled to room temperature. The temperature of the polymerization kettle was set to 80°C, 100mL of toluene solution of norbornene (6M) and 0.4mmol of triisobutylaluminum were added, and the liquid phase and gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of catalyst compound A7 (2μmol / L) and a toluene mixed solution of triphenylcarbon tetrakis (pentafluorophenyl) borate with a 1.1 times equivalent relative to Ti were added, and ethylene was introduced at a pressure of 10atm, and the pressure in the polymerization kettle was maintained at 5atm. The polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 6.71×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 6.57 × 10 5 The glass transition temperature Tg of the copolymer of ethylene and norbornene is 101°C.

[0099] Example 22 Catalyst Compound A3 is used as a catalyst to catalyze ethylene / norbornene copolymerization:

[0100] The polymerization kettle was heated to 120°C, vacuumed and filled with nitrogen repeatedly, and finally the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 80°C, 100mL of toluene solution of norbornene (6M) and 0.4mmol of triisobutylaluminum were added, and the liquid phase and gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of catalyst compound A3 (2μmol / L) and a toluene mixed solution of tri(pentafluorophenyl)borane with a 1.5-fold equivalent relative to Ti were added, and ethylene was introduced at a pressure of 10atm, the pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 4.26×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 4.19 × 10 5 The glass transition temperature Tg of the copolymer of ethylene and norbornene is 88.2°C.

[0101] Example 23 Catalyst Compound A1 is used as a catalyst to catalyze ethylene / 1-octene copolymerization:

[0102] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 140°C, and 70mL toluene, 30mL 1-octene, and 1.5mmol methylaluminoxane were added. The liquid phase and the gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of a toluene solution of the catalyst compound A1 (2μmol / L) was added, and ethylene was introduced at a pressure of 4MPa. The pressure in the polymerization kettle was maintained at 10atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was vacuum dried at 60°C. The polymerization activity of the system was about 8.16×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 6.66 × 10 5 g / mol, and the 1-octene insertion rate in the copolymer is 10.1%.

[0103] Example 24 Catalyst Compound A3 is used as a catalyst to catalyze ethylene / 1-octene copolymerization:

[0104] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 140°C, and 70mL toluene, 30mL 1-octene, and 1.5mmol methylaluminoxane were added. The liquid phase and the gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of a toluene solution of the catalyst compound A3 (2μmol / L) was added, and ethylene was introduced at a pressure of 4MPa. The pressure in the polymerization kettle was maintained at 10atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was vacuum dried at 60°C. The polymerization activity of the system was about 8.4×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 6.73 × 10 5 g / mol, and the 1-octene insertion rate in the copolymer is 12.8%.

[0105] Example 25 Catalyst Compound A4 is used as a catalyst to catalyze ethylene / 1-octene copolymerization:

[0106] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly pumped and filled with nitrogen for several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 140°C, and 70mL of toluene, 30mL of 1-octene, and 1.5mmol of methylaluminoxane were added. The liquid phase and the gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of a toluene solution of the catalyst compound A4 (2μmol / L) was added, and ethylene was introduced at a pressure of 4MPa. The pressure in the polymerization kettle was maintained at 10atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was vacuum dried at 60°C. The polymerization activity of this system was about 2.5×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 1.97 × 10 5 g / mol, and the 1-octene insertion rate in the copolymer is 7.26%.

[0107] Example 26 Catalyst Compound A5 is used as a catalyst to catalyze ethylene / 1-octene copolymerization:

[0108] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 140°C, and 70mL toluene, 30mL 1-octene, and 1.5mmol methylaluminoxane were added. The liquid phase and the gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of a toluene solution of the catalyst compound A5 (2μmol / L) was added, and ethylene was introduced at a pressure of 4MPa. The pressure in the polymerization kettle was maintained at 10atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was vacuum dried at 60°C. The polymerization activity of this system was about 3.1×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 2.77 × 10 5 g / mol, and the 1-octene insertion rate in the copolymer is 7.9%.

[0109] Example 27 Catalyst Compound A7 was used as a catalyst to catalyze ethylene / 1-octene copolymerization:

[0110] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 140°C, and 70mL toluene, 30mL 1-octene, and 1.5mmol methylaluminoxane were added. The liquid phase and the gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of a toluene solution of the catalyst compound A7 (2μmol / L) was added, and ethylene was introduced at a pressure of 4MPa. The pressure in the polymerization kettle was maintained at 10atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was vacuum dried at 60°C. The polymerization activity of the system was about 7.29×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 5.98 × 10 5 g / mol, and the 1-octene insertion rate in the copolymer is 9.48%.

[0111] Comparative Example 1Me5CpTiCl2(O-2,6- i Pr2C6H3) is used as a catalyst to catalyze ethylene polymerization:

[0112] Catalyst Me5CpTiCl2(O-2,6- i Pr2C6H3) was synthesized according to the literature (i.e., the above-mentioned compound b, see Organometallics, 1998, 17(11): 2152-2154).

[0113] The polymerization kettle was heated to 120°C, and the vacuum was repeatedly evacuated and nitrogen was filled several times. Finally, the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 25°C, 100mL of toluene and 2mmol of methylaluminoxane were added, and the liquid phase and the gas phase were saturated with ethylene gas at 25°C. Subsequently, 1mL of a toluene solution of compound b (2μmol / L) was added, and ethylene was introduced at a pressure of 5atm. The pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 15min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 3.7×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 2.15 × 10 5 g / mol.

[0114] Comparative Example 2Me5CpTiCl2(O-2,6-i Pr2C6H3) is used as a catalyst to catalyze ethylene / norbornene copolymerization:

[0115] The polymerization kettle was heated to 120°C, vacuumed and filled with nitrogen several times, and finally the nitrogen was replaced with ethylene, and the temperature was lowered to room temperature. The temperature of the polymerization kettle was set to 80°C, 100mL of toluene solution of norbornene (6M) and 0.4mmol of triisobutylaluminum were added, and the liquid phase and gas phase were saturated with ethylene gas at 25°C. After heating to the set temperature, 1mL of compound b (2μmol / L) and a toluene mixed solution of triphenylcarbon tetrakis (pentafluorophenyl) borate with a 1.1 times equivalent relative to Ti were added, and ethylene was introduced at a pressure of 10atm, the pressure in the polymerization kettle was maintained at 5atm, and the polymerization time was 10min. After the polymerization reaction was completed, 1mL of ethanol was added to terminate the reaction, and the reaction product was poured into 200mL of acidified ethanol (containing 10% by volume of hydrochloric acid), filtered, and washed three times with 100mL of ethanol. The obtained polymer was dried to constant weight under vacuum at 60°C. The polymerization activity of this system is about 4.58×10 6 g polymer / (mol Ti h), polymer molecular weight Mw = 3.72 × 10 5 The glass transition temperature Tg of the copolymer of ethylene and norbornene is 68°C.

[0116] It can be seen from the results of Comparative Example 1 and Example 9 that when the olefin polymerization catalyst provided by the present invention catalyzes ethylene polymerization, under the same polymerization conditions, the polymerization activity is relatively higher, and the molecular weight of the obtained polymer is larger; it can be seen from the results of Comparative Example 2 and Example 17 that when the olefin polymerization catalyst provided by the present invention catalyzes the copolymerization of ethylene and norbornene, under the same polymerization conditions, the polymerization activity is relatively higher, the molecular weight of the obtained copolymer is larger, and the glass transition temperature of the copolymer is also higher, indicating that the norbornene insertion rate is also higher. It can be seen that the olefin polymerization catalyst of the present invention has better comprehensive catalytic performance and has more application prospects.

[0117] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A catalyst compound, characterized in that The structural formula of the compound is:

2. A catalyst for olefin polymerization, characterized in that A catalyst compound according to any one of claims 1.

3. The catalyst for olefin polymerization according to claim 2, characterized in that The olefin polymerization catalyst also includes alkylaluminoxane as a co-catalyst, and / or a combination of alkylaluminum and an organic boron compound as a co-catalyst to form a catalyst system together with the catalyst compound.

4. The catalyst for olefin polymerization according to claim 3, characterized in that The alkylaluminoxane is methylaluminoxane, ethylaluminoxane, isobutylaluminoxane or alkyl-modified methylaluminoxane; the alkylaluminum is trimethylaluminum, triethylaluminum or triisobutylaluminum; the organic boron compound is tris(pentafluorophenyl)borane, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate or N,N-dimethylbenzylammonium tetrakis(pentafluorophenyl)borate.

5. The catalyst for olefin polymerization according to claim 3, characterized in that The molar ratio of the catalyst compound to the alkylaluminoxane is 1:50-20000, wherein the molar amounts of titanium and aluminum are used respectively; the molar ratio of the catalyst compound to the alkylaluminum and organic boron compound composition is 1:50-20000:1-3, wherein the molar amounts of titanium, aluminum and boron are used respectively.

6. Use of a catalyst for olefin polymerization according to any one of claims 2 to 5, characterized in that Used to catalyze the homopolymerization of ethylene and / or the copolymerization of ethylene and α-olefins / cycloolefins.

Citation Information

Patent Citations

  • Preparation method and application of half- metallocene catalyst

    CN113248548A