A multi-component organic semiconductor material and its preparation method and application

Through the network structure and simple preparation method of multi-component organic semiconductor materials, the problem of heterojunction aging in organic photovoltaic cells is solved, the stability and efficiency are improved, the production process is simplified, and high-performance photovoltaic cells are realized.

CN115651169BActive Publication Date: 2024-11-26GUANGZHOU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211207330.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-26
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

In organic photovoltaic cells, based on the aging problem of the film morphology of the bulk heterojunction blended by electron donor and electron acceptor under conditions such as light and heating, it is extremely difficult to synthesize and separate existing high-performance single-component photovoltaic materials. Large, difficult to balance efficiency and stability.

Method used

Using multi-component organic semiconductor materials, a network structure interspersed through PM6, L15, PM6-b-L15 is formed to fill the gaps to improve material stability. A simple one-pot method is used to prepare the photoactivity of organic photovoltaic cells. layer.

Benefits of technology

It improves the stability of the material and the aging resistance of photovoltaic cells, simplifies the production process, reduces costs and time, and improves the applicability of industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention discloses a multi-component organic semiconductor material and a preparation method and application thereof. A multi-component organic semiconductor material comprises PM6, L15, and PM6-b-L15, wherein PM6, L15, and PM6-b-L15 form a mutually interpenetrating network structure. The multi-component organic semiconductor material of the invention adopts PM6, L15, and PM6-b-L15 to form a mutually interpenetrating network structure, wherein PM6 and L15 can be filled into the gaps of PM6-b-L15 to form a more compact stacking, thereby improving the stability of the material. When the material is used as a photoactive layer in an organic photovoltaic cell, the material has stable properties and is resistant to aging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organic semiconductor materials, and in particular to a multi-component organic semiconductor material and a preparation method and application thereof. Background Art

[0002] In organic photovoltaic cells, the aging of the film morphology of the bulk heterojunction based on the blend of electron donors and electron acceptors under conditions such as light and heating is a major challenge facing the practical application of organic photovoltaic technology. Photovoltaic materials based on organic semiconductors are the core of the development of organic photovoltaic technology. At present, starting from photovoltaic materials, different methods are used to improve the morphological stability, such as the use of all-polymer bulk heterojunctions, single-component active layers, etc. The construction of high-performance single-component photovoltaic materials provides an effective way to solve this problem, but the synthesis and separation of high-performance single-component photovoltaic materials are extremely difficult, and it is difficult to balance the efficiency and stability of organic photovoltaic cells. Summary of the invention

[0003] In order to overcome the aging problem of existing photovoltaic materials, the purpose of the present invention is to provide a multi-component organic semiconductor material. The second purpose of the present invention is to provide a method for preparing the multi-component organic semiconductor material. The third purpose of the present invention is to provide an application of the multi-component organic semiconductor material.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A multi-component organic semiconductor material, the multi-component organic semiconductor material comprises PM6, L15, and PM6-b-L15, wherein PM6, L15, and PM6-b-L15 form a mutually interpenetrating network structure;

[0006] The structural formula of PM6 is as follows:

[0007]

[0008] The structural formula of the L15 is as follows:

[0009]

[0010] The structural formula of PM6-b-L15 is as follows:

[0011]

[0012] In the formula, m:n=1:1.

[0013] Preferably, in this multi-component organic semiconductor material, the mass ratio of PM6, L15, and PM6-b-L15 is (1-10):(1-10):100.

[0014] Preferably, in the multi-component organic semiconductor material, the molecular weight of the multi-component organic semiconductor material is 15-60 kDa; further preferably, the molecular weight of the multi-component organic semiconductor material is 20-55 kDa.

[0015] The second aspect of the present invention provides a method for preparing the above-mentioned multi-component organic semiconductor material, comprising the following steps:

[0016] Mixing a1, d1, a2 and a3 in a solvent for reaction to obtain the multi-component organic semiconductor material;

[0017] The structural formula of a1 is as follows:

[0018]

[0019] The structural formula of d1 is as follows:

[0020]

[0021] The structural formula of a2 is as follows:

[0022]

[0023] The structural formula of a3 is as follows:

[0024]

[0025] Preferably, in the method for preparing the multi-component organic semiconductor material, the reaction temperature is 100-120°C; further preferably, the reaction temperature is 105-115°C.

[0026] Preferably, in the preparation method of this multi-component organic semiconductor material, a1 and d1 are first mixed and reacted for 1-3 hours, and then a2 and a3 are added and mixed and reacted for 20-28 hours; further preferably, a1 and d1 are first mixed and reacted for 1.5-2.5 hours, and then a2 and a3 are added and mixed and reacted for 22-26 hours.

[0027] Preferably, in the preparation method of this multi-component organic semiconductor material, the molar mass ratio of a1, d1, a2, and a3 is 1: (0.8-1.2): (0.8-1.2): (0.8-1.2); further preferably, the molar mass ratio of a1, d1, a2, and a3 is 1: (0.9-1.1): (0.9-1.1): (0.9-1.1); in some preferred specific embodiments of the present invention, the molar mass ratio of a1, d1, a2, and a3 is 1:1:1:1.

[0028] Preferably, in the preparation method of the multi-component organic semiconductor material, a1, d1, a2 and a3 are mixed and reacted, and then precipitated with alcohol and filtered to obtain a crude product, and the crude product is purified to obtain the multi-component organic semiconductor material.

[0029] Preferably, in the method for preparing the multi-component organic semiconductor material, the solvent is toluene.

[0030] The third aspect of the present invention provides a photoactive layer comprising the above-mentioned multi-component organic semiconductor material.

[0031] A fourth aspect of the present invention provides use of the multi-component organic semiconductor material in the preparation of an organic photovoltaic cell.

[0032] The beneficial effects of the present invention are:

[0033] The multi-component organic semiconductor material of the present invention adopts PM6, L15, and PM6-b-L15 to form an interpenetrating network structure. PM6 and L15 can be filled into the gaps of PM6-b-L15 to form a tighter stacking, thereby improving the stability of the material. When the material is used as a photoactive layer of an organic photovoltaic cell, the material has stable properties and is resistant to aging.

[0034] The preparation method of the multi-component organic semiconductor material of the present invention is simple and the preparation raw materials are easily available. When the material is used as the photoactive layer of an organic photovoltaic cell, the production cost and time of the organic photovoltaic material can be effectively reduced, the stability of the organic photovoltaic cell can be improved, and industrialization is facilitated.

[0035] The method for preparing the multi-component organic semiconductor material of the present invention adopts a one-pot preparation method, which is simple and easy to operate and does not require a complicated post-processing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Schematic diagram of the process of preparing organic semiconductor materials in the embodiment.

[0037] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of compound a2 prepared in Example 1.

[0038] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of compound a3 prepared in Example 1.

[0039] Figure 4 This is the NMR image of the multi-component organic semiconductor material S11 prepared in Example 1.

[0040] Figure 5 This is the hydrogen nuclear magnetic resonance spectrum of compound L15 prepared in Example 2.

[0041] Figure 6 It is the NMR comparison diagram of the embodiment.

[0042] Figure 7 F and N elemental analysis diagrams of the materials prepared in Example 1 and Example 4.

[0043] Figure 8 This is a stability comparison diagram of the multi-component organic semiconductor material S11 and the binary component PM6:L15.

[0044] Fig. 9 Photovoltaic stability data of the multi-component organic semiconductor material S11 prepared in Example 1 and the binary component PM6:L15 prepared in Example 3.

[0045] Fig.10 Photovoltaic performance parameters of the multi-component organic semiconductor material S11 prepared in Example 1 and the binary component PM6:L15 prepared in Example 3. DETAILED DESCRIPTION

[0046] The present invention is further described in detail below through specific examples. It should be noted that the following examples do not limit the scope of protection claimed by the present invention.

[0047] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0048] Example 1

[0049] This embodiment provides a method for preparing a multi-component organic semiconductor material. Figure 1 The synthesis route of the multi-component organic semiconductor shown in the figure specifically includes the following steps:

[0050] 1) Preparation of compound a2, the specific steps are as follows:

[0051] Under argon protection, compound b (200 mg, 0.14 mmol), IC-Br (159.6 mg, 0.6 mmol), pyridine (1 mL) and chloroform (25 mL) were added to a flask, and the reaction was stirred at 65 ° C for 12 hours. After cooling to room temperature, the mixture was poured into methanol and filtered. The residue was purified by column chromatography on silica gel using a mixed solvent of dichloromethane and petroleum ether as an eluent to obtain a dark blue solid, which was the product Y5-Br, i.e., a2 (209 mg, 80% yield).

[0052]

[0053] 2) Preparation of compound a3, the specific steps are as follows:

[0054] Dissolve dithiophene imide (BTI) (460 mg, 1.00 mmol) in 10 mL of tetrahydrofuran, and add fresh LDA (2.5 mL, 2.1 mmol) dropwise at low temperature. Stir the reaction mixture at low temperature for 1 hour, add a THF solution of (n-Bu)3SnCl (0.7 mL, 2.20 mmol) to the reaction at -78°C for 1 hour, and then slowly warm the reaction mixture to ambient temperature and stir at this temperature overnight. Quench the reaction mixture with 40 mL of H2O and extract with CHCl3 (3×50 mL), then wash with saturated aqueous NaHCO3 (20 mL) and H2O (40 mL), combine the organic layers, and dry them over anhydrous Na2SO4. After removing the solvent under vacuum, the residue is purified by flash column chromatography on silica gel with petroleum ether as the eluent to obtain the monomer BTI-Tin a3 (622 mg, 60%) as a colorless oil.

[0055]

[0056] 3) Preparing a multi-component organic semiconductor material, the specific steps are as follows:

[0057] d1 (477.79 mg, 0.05 mmol), a1 (383.36 mg, 0.05 mmol) and Pd (PPh3) 4 (4 mg) were placed in a reactor, 5 mL of toluene was added, the reaction temperature was set to 110 ° C, and PM6 was obtained after two hours of reaction. A toluene solution of a2 (937.21 mg, 0.05 mmol) and a3 (548.80 mg, 0.05 mmol) was added to the reactor and reacted for 24 hours. After the reaction, the temperature was lowered to room temperature, the reaction solution was poured into methanol for precipitation, filtered, and dried, the crude product was dissolved in chloroform, and S11 (multi-component organic semiconductor material) was collected after rapid column chromatography, concentrated and precipitated, and dried in a vacuum oven. The molecular weight and molecular weight distribution of S11 were Mn = 18.6 kDa, Mw = 50.4 kDa, and PDI = 2.71.

[0058] The above d1 and a1 were purchased from Shuolun Organic Optoelectronics Technology Co., Ltd.

[0059] The hydrogen nuclear magnetic resonance spectrum of the compound a2 prepared above is as follows: Figure 2 shown.

[0060] The hydrogen nuclear magnetic resonance spectrum of the compound a3 prepared above is as follows: Figure 3 shown.

[0061] The NMR image of the multi-component organic semiconductor material S11 prepared above is as follows: Figure 4 shown.

[0062] In addition, two sets of experiments were repeated according to the above experimental conditions, and the final molecular weights of S11 were 30.7 kDa and 25.3 kDa, respectively.

[0063] Example 2

[0064] Reference Figure 1 This embodiment provides a method for preparing compound L15, which specifically comprises the following steps:

[0065] The toluene solution of a2 (937.21 mg, 0.5 mmol) and a3 (548.80 mg, 0.5 mmol) prepared in Example 1 was added to the reactor and reacted for 24 hours. After the reaction, the temperature was lowered to room temperature, the reaction solution was poured into methanol for precipitation, filtered, and dried, the crude product was dissolved in chloroform, and after rapid column chromatography, L15 was collected, concentrated and precipitated, and dried in a vacuum oven.

[0066] The hydrogen nuclear magnetic resonance spectrum of compound L15 prepared in this example is as follows Figure 5 shown.

[0067] Example 3

[0068] In this example, the compound PM6 prepared in Example 1 and the compound L15 prepared in Example 2 were physically mixed at room temperature in a mass ratio of 1:1 to obtain a mixture named PM6:L15.

[0069] Example 4

[0070] The multi-component organic semiconductor material S11 prepared in Example 1 was subjected to column chromatography and then Soxhlet extraction (the extraction solvents were methanol, acetone, petroleum ether, and dichloromethane for 12 hours each, and then chloroform was used for Soxhlet extraction for 4 hours to obtain a chloroform solution of PM6-b-L15, which was concentrated to 10 mL and then added with methanol for precipitation and filtration to obtain compound PM6-b-L15.

[0071] The NMR comparison images of S11 prepared in Example 1, PM6 prepared in Example 1, L15 prepared in Example 2, PM6:L15 prepared in Example 3 and PM6-b-L15 prepared in Example 4 are shown in FIG. Figure 6 shown.

[0072] The F and N elemental analysis of S11 prepared in Example 1 and PM6-b-L15 prepared in Example 4 is as follows: Figure 7 shown.

[0073] The multi-component organic semiconductor material S11 prepared in Example 1 and the binary component PM6:L15 prepared in Example 3 were placed at room temperature for 1000 hours. The morphology of the materials before and after the placement is compared as shown in the attached figure. Figure 8 As shown in the attached Figure 8It can be seen that the binary component PM6:L15 shows serious aggregation after long-term storage, while the multi-component S11 still maintains a good interpenetrating network structure after long-term storage. PM6 and L15 fill the gaps of PM6-b-L15 to achieve a tighter stacking.

[0074] The stability test of the organic photovoltaic device of the multi-component organic semiconductor material S11 prepared in Example 1 and the binary component PM6:L15 prepared in Example 3 is as follows: Fig. 9 The photovoltaic performance parameters are shown in Fig.10 As shown; Fig. 9 Figure a in the figure shows the stability test data of S11 and PM6:L15 over time when placed at room temperature; Fig. 9 Figure b in the figure shows the stability test data of S11 and PM6:L15 when placed at room temperature and irradiated with white light over time; Fig. 9 Figure c in the figure shows the stability test data of S11 and PM6:L15 over time when placed at 85°C. Fig. 9 It can be seen from the data that the S11 stability of the organic photovoltaic device based on the heterojunction of multi-component organic semiconductors prepared in Example 1 is greatly improved compared with the traditional binary system PM6:L15.

[0075] from Fig.10 It can be seen that S11 still maintains the high voltage of PM6:L15.

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A multi-component organic semiconductor material, characterized in that: The multi-component organic semiconductor material comprises PM6, L15, PM6- b -L15, PM6, L15, PM6- b -L15 forms an interlaced network structure; The structural formula of PM6 is as follows: ; The structural formula of the L15 is as follows: ; The PM6- b -L15 has the following structural formula: ; Wherein, m:n=1:1; The molecular weight of the multi-component organic semiconductor material is 15-60 kDa.

2. The multi-component organic semiconductor material according to claim 1, characterized in that: PM6, L15, PM6- b -The mass ratio of L15 is (1-10):(1-10):

100.

3. A method for preparing a multi-component organic semiconductor material according to any one of claims 1 to 2, characterized in that: The following steps are involved: Mixing a1, d1, a2 and a3 in a solvent for reaction to obtain the multi-component organic semiconductor material; The structural formula of a1 is as follows: ; The structural formula of d1 is as follows: ; The structural formula of a2 is as follows: ; The structural formula of a3 is as follows: 。 4. The method for preparing a multi-component organic semiconductor material according to claim 3, characterized in that: The reaction temperature is 100-120°C.

5. The method for preparing a multi-component organic semiconductor material according to claim 3, characterized in that: The a1 and d1 are first mixed and reacted for 1-3 hours, and then a2 and a3 are added and mixed and reacted for 20-28 hours.

6. The method for preparing a multi-component organic semiconductor material according to claim 3, characterized in that: The molar mass ratio of a1, d1, a2 and a3 is 1:(0.8-1.2):(0.8-1.2):(0.8-1.2).

7. The method for preparing a multi-component organic semiconductor material according to claim 3, characterized in that: After the a1, d1, a2 and a3 are mixed for reaction, the mixture is precipitated with alcohol and filtered to obtain a crude product, and the crude product is purified to obtain the multi-component organic semiconductor material.

8. A photoactive layer, characterized in that The invention comprises the multi-component organic semiconductor material according to any one of claims 1 to 2.

9. Use of the multi-component organic semiconductor material according to any one of claims 1 to 2 in the preparation of an organic photovoltaic cell.