A self-cleaning epoxy seam beautifying agent and preparation method thereof
Through the combination of silicon-modified epoxy resin and amino-modified nanofiller, a cross-linking network structure is formed, which solves the harmful problem of fluorine in existing self-cleaning seam beautifiers, and realizes the self-cleaning and multi-functional application of seam beautifiers. , extends service life and reduces environmental and human hazards.
Patent Information
- Application Number
- CN202211373688.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-03
AI Technical Summary
The introduction of a large amount of fluorine elements in existing self-cleaning and sewing agents is harmful to the environment and the human body, and is difficult to apply on a large scale. In addition, traditional cement-based sewing agents are prone to contamination and have a short service life.
Silicon modified epoxy resin is used to reduce the surface energy of the seam-applied agent, combine amino-modified nanofillers and ultraviolet absorbers to form a crosslinking network structure, realize surface hydrophobic characteristics and photodegradation functions, and avoid contamination.
It realizes the self-cleaning function of the seam surface, extends the service life, improves multi-functional applications, and reduces environmental and human body hazards, and enhances yellowing resistance and air purification performance.
Smart Images

Figure CN115651495B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coatings, and more specifically, relates to a self-cleaning epoxy seam beautifying agent and a preparation method thereof. Background Art
[0002] Traditionally, the research and application of tile caulking materials are mostly cement-based caulking agents, which can meet the basic needs of caulking and are relatively cheap, but are very easy to be contaminated, blackened, cracked, or even fall off after long-term use. In recent years, with the improvement of living standards, consumers have put forward higher requirements for color decoration, multi-function, and high performance. Two-component epoxy-based caulking agents are widely favored by consumers due to their high hardness, strong adhesion, mildew and antibacterial, high and low temperature resistance, and rich colors.
[0003] Sealing agents are in contact with many household appliances, and light-colored surfaces are easily contaminated, which particularly affects the appearance. Therefore, if a self-cleaning seaming agent product can be developed, the service life of the seaming agent can be greatly extended, its maintenance time can be saved, and the multifunctional application of the seaming agent can also be broadened. The Chinese invention patent application CN113185897A discloses a super-hydrophobic self-cleaning seaming agent, which mainly reduces the surface energy by fluorine-containing epoxy resin, and obtains the surface roughness by fluorine-modified nano-silica. The combination of low surface energy and roughness realizes the super-hydrophobicity of the material surface, thereby realizing the self-cleaning function. However, the introduction of a large amount of fluorine elements will cause great harm to the environment and the human body, which is not conducive to large-scale application.
[0004] Therefore, it is urgent to propose a new self-cleaning epoxy seam beautifying agent and a preparation method thereof. Summary of the invention
[0005] The purpose of the present invention is to provide a self-cleaning epoxy caulking agent and a preparation method thereof in view of the deficiencies of the prior art. The present invention reduces the surface energy of the caulking agent by introducing silicon-modified epoxy resin, so that the surface of the caulking agent presents hydrophobic properties, and common pollutants are sprinkled on the surface of the caulking agent in the form of droplets, which are not easy to wet the surface.
[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a self-cleaning epoxy seam beautifying agent, which comprises a component A and a component B;
[0007] The component A comprises: an epoxy resin mixture, a diluent and fumed silica;
[0008] The B component includes: fumed silica, a curing agent, a defoaming agent, a thickening thixotropic agent, an ultraviolet absorber, a pigment and an amino-modified nano filler;
[0009] The epoxy resin mixture comprises: bisphenol A epoxy resin, bisphenol F epoxy resin and silicon-modified epoxy resin.
[0010] According to the present invention, preferably, the component A comprises the following components in parts by weight: 80-90 parts of epoxy resin mixture, 1-10 parts of diluent and 3-10 parts of fumed silica;
[0011] The B component includes the following components in parts by weight: 2-10 parts of fumed silica, 60-90 parts of curing agent, 0.1-1 parts of defoaming agent, 0.5-2 parts of thickening thixotropic agent, 0.1-2 parts of ultraviolet absorber, 1-5 parts of pigment and 1-10 parts of amino-modified nano filler.
[0012] According to the present invention, preferably, the mass ratio of the bisphenol A epoxy resin, the bisphenol F epoxy resin and the silicon-modified epoxy resin is (70-90):(2-7):1.
[0013] According to the present invention, preferably, the bisphenol A epoxy resin is at least one of E51 epoxy resin, E44 epoxy resin, 2,2-bis(4-glycidyloxyphenyl)propane, 2-[1-[4-[2-[2-(oxyethylethoxy)propoxy]phenyl]prop-2-yl]phenoxy]prop-2-ethylmethyl]oxyethane and 2-[[4-[bis[4-(oxy-2-methoxy)phenyl]methyl]phenoxy]methyl]oxyethane.
[0014] According to the present invention, preferably, the bisphenol F epoxy resin is at least one of NPEF-170 epoxy resin, NPEF-164X epoxy resin, NPEF-171 epoxy resin, NPEF-175 epoxy resin, NPEF-198 epoxy resin, NPEF-500 epoxy resin and bis(4-glycidyloxyphenyl)methane.
[0015] According to the present invention, preferably, the silicon-modified epoxy resin is at least one of trimethyl-[methyl-bis[1-(oxiran-2-yl)butyl]silyl]oxysilane, 4-(oxiran-2-yl)butyl-[4-(oxiran-2-yl)butyl-dipropylsilyl]oxydipropylsilane, trimethyl-[methyl-bis[1-(oxiran-2-yl)butyl]silyl]oxysilane and [3,3-bis(oxan-2-methoxy)propyl-methylsilyl]oxytrimethylsilane.
[0016] In the present invention, a large number of hydroxyl groups exist on the surface of the fumed silica, which can form hydrogen bonds with the epoxy resin to form a three-dimensional network structure, play a role as a skeleton, and improve the sagging performance of the seam beautifying agent.
[0017] According to the present invention, preferably, the diluent is at least one of benzyl alcohol, N,N-dimethylformamide, tetrahydrofuran and xylene.
[0018] According to the present invention, preferably, the curing agent is at least one of 1,3-cyclohexanedimethylamine, 5-amino-1,3,3-trimethylcyclohexylmethylamine, 3-[3-(aminomethyl)cyclohexyl]propylamine, 3-[4-(aminomethyl)cyclohexyl]propylamine, 3-[3-(3-aminopropyl)cyclohexyl]-1-propylamine, [3-(aminomethyl)-3-methylcyclohexyl]methylamine, 4-[3,5-bis(4-aminobutyl)cyclohexyl]butylamine, [3-(aminomethyl)-5-methylcyclohexyl]methylamine, 2-[3,5-bis(2-aminoethyl)cyclohexyl]ethylamine, [3-(aminomethyl)-3,5,5-trimethylcyclohexyl]methylamine and 2-(3-(aminomethyl)cyclohexyl)ethylamine.
[0019] According to the present invention, preferably, the defoamer is a silicone defoamer, preferably at least one of BYK-141, BYK-A530, BYK-020, BYK-022, BYK-024 and BYK-028.
[0020] In the present invention, the thickening thixotropic agent cooperates with fumed silica to ensure the construction performance of the product. According to the present invention, preferably, the thickening thixotropic agent is at least one of wx-552 flow stopper, BYK-R607 flow stopper, and 8610 flow stopper. The thickening thixotropic agent is at least one of wx-552 flow stopper, BYK-R607 flow stopper, and 8610 flow stopper.
[0021] According to the present invention, preferably, the ultraviolet absorber is at least one of 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-octoxyphenol, 4-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]benzene-1,3-diol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-pentadecylphenol, 2-[4,6-bis(3-ethyl-2-hydroxyphenyl)-1,3,5-triazine-2-yl]-6-ethylphenol and 4-[4-(2,4-dimethylphenyl)-6-(2-hydroxyphenyl)-1,3,5-triazine-2-yl]benzene-1,3-diol.
[0022] According to the present invention, preferably, the amino-modified nanofiller is obtained by surface grafting modification of the filler with γ-aminopropyltriethoxysilane.
[0023] According to the present invention, preferably, the filler is at least one of nano titanium dioxide, nano zinc oxide, nano tin oxide and nano zirconium dioxide.
[0024] According to the present invention, preferably, the method for preparing the amino-modified nanofiller comprises:
[0025] (1) mixing the filler with ethanol and stirring to disperse them uniformly to obtain a first mixed solution;
[0026] (2) uniformly mixing the γ-aminopropyltriethoxysilane and water to obtain a second mixed solution;
[0027] (3) The first mixed solution and the second mixed solution are mixed and stirred for reaction, centrifuged, washed, and dried to obtain the amino-modified nanofiller.
[0028] According to the present invention, preferably, in step (1), the ratio of the filler to ethanol is 1: (9-12) g / mL;
[0029] In step (2), the ratio of γ-aminopropyltriethoxysilane to water is 1: (120-200) g / mL;
[0030] In step (3), the temperature of the mixed stirring reaction is 50-100° C. and the time is 2-12 hours; the washing method includes: washing with water and / or ethanol.
[0031] In the present invention, the surface of the nanofiller is grafted and modified by γ-aminopropyltriethoxysilane, so that it is not simply blended and dispersed in the formula system, but the surface amino group reacts with the epoxy group to finally form a cross-linked network structure of epoxy resin and nanofiller. On this basis, since the nanofiller has a photodegradation function, after the surface is contaminated, after being exposed to light, the pollutants on the surface can be easily decomposed into inorganic substances such as water and carbon dioxide, and common gas pollutants in the room can also be degraded to achieve indoor air purification.
[0032] According to the present invention, preferably, the mass ratio of the component A to the component B is 1:(0.7-1.3).
[0033] In the present invention, the pigment is one or more of toner or color paste.
[0034] In the present invention, the fumed silica is a synthetic amorphous silica gel known to those skilled in the art.
[0035] The second aspect of the present invention provides a method for preparing the self-cleaning epoxy seam beautifying agent, the method comprising the following steps:
[0036] S1: mixing and stirring the epoxy resin mixture with a diluent to obtain an epoxy resin mixed liquid; mixing and stirring the epoxy resin mixed liquid with fumed silica to obtain the component A by vacuum degassing;
[0037] S2: The curing agent, defoaming agent, fumed silica, pigment, amino-modified nanofiller, thickening thixotropic agent and ultraviolet absorber are mixed and stirred uniformly, and vacuumed to degas to obtain the B component.
[0038] The beneficial effects of the technical solution of the present invention are as follows:
[0039] 1) The caulking agent of the present invention is a two-component epoxy caulking agent, and therefore has the advantages of high mechanical strength, strong adhesion, and high heat resistance, which are common to epoxy resins. At the same time, the caulking agent of the present invention greatly improves the flexibility of the cured product by introducing the ether bond flexible chain in the bisphenol F epoxy resin and the toughening effect of the diluent (preferably benzyl alcohol). At the same time, the introduction of the silicon-modified epoxy resin reduces the surface energy of the caulking agent, making its surface hydrophobic. Common pollutants are sprinkled on the surface of the caulking agent in the form of droplets, and it is not easy to wet its surface.
[0040] 2) The curing agent of the present invention is a modified alicyclic amine curing agent, which does not contain aromatic groups that are prone to yellowing, so it is not easy to undergo photochemical reactions to cause degradation. In addition, the ultraviolet light absorption and reflection of the ultraviolet light by the ultraviolet absorber and the amino-modified nano-filler (preferably amino-modified nano-titanium dioxide) greatly improve the yellowing resistance of the seam beautifying agent.
[0041] 3) The present invention uses γ-aminopropyltriethoxysilane to graft and modify the surface of the nanofiller, thereby improving its dispersibility in the seam beautifier and reducing the agglomeration between particles. In addition, the amino-modified nanofiller can directly react chemically with the epoxy resin (surface amino groups react with epoxy groups), thereby improving the hardness and impact resistance of the seam beautifier.
[0042] 4) Due to the introduction of fillers such as nano titanium dioxide, nano zinc oxide, nano tin oxide and nano zirconium dioxide, when the surface of the caulking agent is contaminated by some pollutants, the photodegradation of fillers such as titanium dioxide can degrade them into water, carbon dioxide and other inorganic substances under light, making it easy to achieve self-cleaning of the surface of the caulking agent. It can also degrade common indoor gaseous pollutants such as formaldehyde, toluene and sulfide, etc., play an air purification role, and broaden the multifunctional application of caulking agents.
[0043] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.
[0045] FIG. 1( a ) shows a contact angle photograph of a self-cleaning epoxy seam beautifying agent provided in Example 1 of the present invention.
[0046] FIG. 1( b ) shows a schematic diagram of a self-cleaning epoxy seam sealant provided in Example 1 of the present invention being contaminated and before being exposed to light.
[0047] FIG. 1( c ) shows a schematic diagram of a self-cleaning epoxy seam sealant provided in Example 1 of the present invention after being contaminated and exposed to light. DETAILED DESCRIPTION
[0048] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0049] Example 1
[0050] This embodiment provides a self-cleaning epoxy seam beautifying agent, which includes component A and component B;
[0051] The component A comprises: 90 g of epoxy resin mixture, 3 g of diluent benzyl alcohol and 6 g of fumed silica; the epoxy resin mixture comprises: 86 g of E51 epoxy resin, 3 g of NPEF-170 epoxy resin and 1 g of trimethyl-[methyl-bis[1-(oxiran-2-yl)butyl]silyl]oxysilane.
[0052] The B component includes: 5.5 g of fumed silica, 50 g of 1,3-cyclohexanedimethylamine, 0.5 g of BYK-141 defoamer, 1.81 g of BYK-R607 flow stopper, 0.76 g of 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-octyloxyphenol, 4.6 g of color powder and 2.5 g of amino-modified nano titanium dioxide;
[0053] The preparation method of the amino-modified nano titanium dioxide comprises:
[0054] (1) Take 10 g of nano-titanium dioxide in 100 mL of ethanol and stir for 30 min to make it evenly dispersed;
[0055] (2) Take 0.2 g of γ-aminopropyltriethoxysilane and dissolve it in 30 mL of water;
[0056] (3) Mixing step (1) and (2), stirring and reacting at 80° C. for 6 h;
[0057] (4) centrifugally precipitating the obtained product, washing it with water and ethanol, and then drying it to obtain amino-modified nano-titanium dioxide.
[0058] The mass ratio of the A component to the B component is 1:1.
[0059] The preparation method of the above-mentioned self-cleaning epoxy seam beautifying agent comprises the following steps:
[0060] S1: Put the above-mentioned bisphenol A epoxy resin, bisphenol F epoxy resin and silicon-modified epoxy resin in a dispersion barrel respectively, add diluent benzyl alcohol, start stirring, adjust the speed to 500r / min, stir for 10 minutes, wait until the resin is completely dissolved, turn off stirring, and obtain an epoxy resin mixed liquid; mix the epoxy resin mixed liquid with fumed silica, start stirring, adjust the speed to 800r / min, stir for 20 minutes, maintain the speed at 800r / min, and degas under vacuum conditions for 30 minutes to obtain component A;
[0061] S2: Add the curing agent and defoaming agent into the dispersion barrel, start stirring, adjust the speed to 500r / min, stir for 10 minutes, wait until the curing agent is dispersed, and then turn off the stirring; continue to add fumed silica to the mixed solution of the curing agent and the defoaming agent in the dispersion barrel, start stirring, adjust the speed to 800r / min, stir for 20 minutes, wait until the fumed silica is completely dispersed, and then turn off the stirring; continue to add color powder and amino-modified nano titanium dioxide, start stirring, maintain the speed at 800r / min, stir for 10 minutes, and then turn off the stirring; add thickening thixotropic agent and ultraviolet absorber, and vacuum degas for 10 minutes to obtain component B.
[0062] S3: Components A and B are fully mixed at a ratio of 1:1, and cured at ambient temperature for 24 hours to obtain the self-cleaning epoxy seam beautifying agent.
[0063] The self-cleaning test of the self-cleaning epoxy caulking agent sample of this embodiment was carried out: the A and B components were fully mixed at a ratio of 1:1, and prepared into a round cake-shaped sample, which was cured at room temperature for 24 hours. When water was dropped on its surface, it showed hydrophobic properties, and the static contact angle was greater than 90°. The contact angle photo is shown in Figure 1 (a). The surface was contaminated with liquids such as juice and cola, which could be easily wiped off with a rag. The stains remaining on the surface could also be easily degraded after 1 day of illumination, restoring the original color and morphology. The photos before and after illumination are shown in Figures 1 (b) and (c): It proves that the caulking agent of the present invention has the function of photodegradation and self-cleaning.
[0064] The hardness test of the self-cleaning epoxy caulking agent sample of this embodiment was performed, and the Shore hardness was 65D.
[0065] Example 2
[0066] This embodiment provides a self-cleaning epoxy seam beautifying agent. The difference between this embodiment and embodiment 1 is that the amino-modified nano titanium dioxide in the B component is 5 g, and other conditions and steps remain unchanged.
[0067] The self-cleaning test results of this embodiment are the same as those of embodiment 1.
[0068] The hardness test of the self-cleaning epoxy caulking agent sample of this embodiment was performed, and the Shore hardness was 67D.
[0069] Example 3
[0070] This embodiment provides a self-cleaning epoxy caulking agent. The difference between this embodiment and embodiment 1 is that the amount of NPEF-170 epoxy resin is 6 g, and other conditions and steps remain unchanged.
[0071] The self-cleaning test results of this embodiment are the same as those of embodiment 1.
[0072] The hardness test of the self-cleaning epoxy caulking agent sample of this embodiment was performed, and the Shore hardness was 64D.
[0073] Example 4
[0074] This embodiment provides a self-cleaning epoxy caulking agent. The difference between this embodiment and embodiment 1 is that the amount of silicon-modified epoxy resin is 2 g, and other conditions and steps remain unchanged.
[0075] The self-cleaning test results of this embodiment are the same as those of embodiment 1.
[0076] The hardness test of the self-cleaning epoxy caulking agent sample of this embodiment was performed, and the Shore hardness was 65D.
[0077] Comparative Example 1
[0078] This comparative example provides a self-cleaning epoxy caulking agent. The difference between this comparative example and Example 1 is that amino-modified nano titanium dioxide is not added, and other conditions and steps remain unchanged.
[0079] The self-cleaning test method of this comparative example is the same as that of Example 1, and the result is that the stains remaining on the surface are not degraded after 1 day of light exposure.
[0080] The hardness test of the self-cleaning epoxy caulking agent sample of this comparative example was performed, and the Shore hardness was 59D.
[0081] Comparative Example 2
[0082] This comparative example provides a self-cleaning epoxy caulking agent. The difference between this comparative example and Example 1 is that no silicon-modified epoxy resin is added, and other conditions and steps remain unchanged.
[0083] The self-cleaning test method of this comparative example is the same as that of Example 1. The results are as follows: after the surface is contaminated by liquids such as juice and cola, the surface is quickly soaked and the contaminants are difficult to wipe off.
[0084] The hardness test of the self-cleaning epoxy caulking agent sample of this comparative example was performed, and the Shore hardness was 61D.
[0085] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A self-cleaning epoxy seam sealant, It is characterized in that The seam beautifying agent comprises component A and component B; The component A comprises the following components in parts by weight: 80-90 parts of epoxy resin mixture, 1-10 parts of diluent and 3-10 parts of fumed silica; The B component includes the following components in parts by weight: 2-10 parts of fumed silica, 60-90 parts of a curing agent, 0.1-1 parts of a defoaming agent, 0.5-2 parts of a thickening thixotropic agent, 0.1-2 parts of an ultraviolet absorber, 1-5 parts of a pigment, and 1-10 parts of an amino-modified nanofiller; The epoxy resin mixture comprises: bisphenol A epoxy resin, bisphenol F epoxy resin and silicon-modified epoxy resin; The silicon-modified epoxy resin is at least one of trimethyl-[methyl-bis[1-(oxiran-2-yl)butyl]silyl]oxysilane, 4-(oxiran-2-yl)butyl-[4-(oxiran-2-yl)butyl-dipropylsilyl]oxydipropylsilane and [3,3-bis(oxan-2-methoxy)propyl-methylsilyl]oxytrimethylsilane; The diluent is at least one of benzyl alcohol, N,N-dimethylformamide, tetrahydrofuran and xylene; The curing agent is at least one of 1,3-cyclohexyldimethylamine, 5-amino-1,3,3-trimethylcyclohexylmethylamine, 3-[3-(aminomethyl)cyclohexyl]propylamine, 3-[4-(aminomethyl)cyclohexyl]propylamine, 3-[3-(3-aminopropyl)cyclohexyl]-1-propylamine, [3-(aminomethyl)-3-methylcyclohexyl]methylamine, 4-[3,5-bis(4-aminobutyl)cyclohexyl]butylamine, [3-(aminomethyl)-5-methylcyclohexyl]methylamine, 2-[3,5-bis(2-aminoethyl)cyclohexyl]ethylamine, [3-(aminomethyl)-3,5,5-trimethylcyclohexyl]methylamine and 2-(3-(aminomethyl)cyclohexyl)ethylamine; The amino-modified nano filler is obtained by surface grafting modification of a filler with γ-aminopropyltriethoxysilane, and the filler is at least one of nano titanium dioxide, nano zinc oxide, nano tin oxide and nano zirconium dioxide; The mass ratio of the component A to the component B is 1:(0.7-1.3).
2. The self-cleaning epoxy seam sealant according to claim 1, in, The mass ratio of the bisphenol A epoxy resin, the bisphenol F epoxy resin and the silicon-modified epoxy resin is (70-90):(2-7):
1.
3. The self-cleaning epoxy seam beautifying agent according to claim 1, in, The bisphenol A epoxy resin is at least one of E51 epoxy resin, E44 epoxy resin, and 2,2-bis(4-glycidyloxyphenyl)propane; The bisphenol F type epoxy resin is at least one of NPEF-170 epoxy resin, NPEF-164X epoxy resin, NPEF-171 epoxy resin, NPEF-175 epoxy resin, NPEF-198 epoxy resin, NPEF-500 epoxy resin and bis(4-glycidyloxyphenyl)methane.
4. The self-cleaning epoxy seam beautifying agent according to claim 1, in, The defoamer is a silicone defoamer; The thickening thixotropic agent is at least one of wx-552 flow stopper, BYK-R607 flow stopper and 8610 flow stopper; The ultraviolet absorber is at least one of 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-octoxyphenol, 4-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]benzene-1,3-diol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-pentadecylphenol, 2-[4,6-bis(3-ethyl-2-hydroxyphenyl)-1,3,5-triazine-2-yl]-6-ethylphenol and 4-[4-(2,4-dimethylphenyl)-6-(2-hydroxyphenyl)-1,3,5-triazine-2-yl]benzene-1,3-diol.
5. The self-cleaning epoxy seam sealant according to claim 4, in, The defoamer is at least one of BYK-141, BYK-A530, BYK-020, BYK-022, BYK-024 and BYK-028.
6. The self-cleaning epoxy seam sealant according to claim 1, in, The preparation method of the amino-modified nanofiller comprises: Step (1) mixing the filler with ethanol and stirring to disperse them uniformly to obtain a first mixed solution; Step (2) uniformly mixing the γ-aminopropyltriethoxysilane with water to obtain a second mixed solution; Step (3) mixing and stirring the first mixed solution and the second mixed solution, centrifuging, washing and drying to obtain the amino-modified nanofiller.
7. The self-cleaning epoxy seam sealant according to claim 6, in, In step (1), the ratio of the filler to ethanol is 1: (9-12) g / mL; In step (2), the ratio of γ-aminopropyltriethoxysilane to water is 1: (120-200) g / mL; In step (3), the temperature of the mixed stirring reaction is 50-100°C and the time is 2-12 hours; the washing method includes: washing with water and / or ethanol.
8. A method for preparing the self-cleaning epoxy seam beautifying agent according to any one of claims 1 to 7, It is characterized in that The method comprises the following steps: S1: mixing and stirring the epoxy resin mixture with a diluent to obtain an epoxy resin mixed liquid; mixing and stirring the epoxy resin mixed liquid with fumed silica to obtain the component A by vacuum degassing; S2: The curing agent, defoaming agent, fumed silica, pigment, amino-modified nanofiller, thickening thixotropic agent and ultraviolet absorber are mixed and stirred uniformly, and vacuumed to degas to obtain the B component.