A waterproof adhesive layer material suitable for warm-mix thin-layer overlay and a preparation method thereof

The waterproof adhesive layer material prepared by grinding solves the problems of easy bonding, large amount of use and seasonal limitations of the bonding layer material in the construction of temperature-mixed and ultra-thin surfaces, and achieves the convenience and high quality of low-temperature seasonal construction. Adhesion strength reduces costs and equipment requirements.

CN115651568BActive Publication Date: 2024-11-05SOUTHWEST MUNICIPAL ENGINEERING DESIGN & RESEARCH INSTITUTE OF CHINA +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211260368.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-14
Publication Date
2024-11-05
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

In the prior art, the construction of the warm-mixed ultra-thin cover has problems such as easy adhesive wheels, large usage, long waiting time for construction, limited seasonality and openness of construction, insufficient adhesion strength and high equipment cost. , especially during low temperature seasons to build.

Method used

It uses a waterproof adhesive layer material composed of mixed rubber powder, rock asphalt, silicon asphalt, intermediate, dispersant, flame retardant and solvent oil, and is made of ball milling and colloid milling, which has good stability. , good permeability, good adhesion, small seasonal restrictions on construction, and no restrictions on special equipment.

Benefits of technology

It has achieved low usage, non-stick wheels, high adhesion strength, and improved construction convenience. It can be effectively constructed in low-temperature seasons, reduces road maintenance costs and equipment requirements, and improves construction efficiency and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a waterproof adhesive layer material suitable for a warm-mix thin-layer overlay and a preparation method thereof. The adhesive layer material is prepared by using 8%-12% of mixed rubber powder, 3%-4% of rock asphalt, 2% of silicon asphalt, 6% of intermediate, 1%-4% of dispersant, 1.5%-2.5% of flame retardant, 1%-2% of stabilizer and 65%-74.5% of solvent oil as raw materials, and then being processed and ground by ball milling and colloid milling in sequence. The mixed rubber powder is a mixed powder composed of SBS rubber powder and SBR rubber powder in a mass ratio of 2-4:3-6. The intermediate is prepared by using 55% of tung oil, 5% of C9 resin, 5% of C5 resin, 30% of C10 liquid petroleum resin, 3% of acrylic acid and 2% of resin catalyst as raw materials, and reacting in a reactor at a temperature of 150-180°C for 8-12 hours. This special waterproof bonding layer material is not easily carried away by material trucks and paving equipment, has a low usage amount, can be stored for a long period of time, and has the advantages of good stability, good permeability, good adhesion, little seasonal construction restrictions, and no special equipment restrictions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road maintenance, and in particular relates to a waterproof bonding layer material suitable for warm-mix thin-layer overlay and a preparation method thereof. Background Art

[0002] As of 2020, the total mileage of highways in China is 5.1981 million kilometers. The highway density is 54.15 kilometers per 100 square kilometers, an increase of 1.94 kilometers per 100 square kilometers. With the further completion of the national road network construction, the realization of road use functions has gradually shifted from early construction to later maintenance. The road maintenance mileage is 5.144 million kilometers, accounting for 99.0% of the total road mileage. During this period, many road maintenance methods have emerged, among which warm mix ultra-thin overlay is an effective road maintenance technology.

[0003] Warm mix asphalt mixture is a mixture mixing technology with a mixing temperature between hot mix asphalt mixture and cold mix asphalt mixture. On the basis of ensuring that the road performance of the asphalt mixture is not affected, the mixing and paving temperature of the asphalt mixture is reduced by about 30°C by reducing the mixing and rolling viscosity of the asphalt mixture during the construction process. Thin layer overlay is a layer of hot mix asphalt mixture with a thickness of not less than 2.5cm laid on the original asphalt pavement. It is usually used for preventive maintenance of roads or treatment of light and medium road diseases. By repairing road surface defects, the original road surface flatness is improved, noise and emission are reduced, and the vibration damage of vehicles to the road surface is reduced, and the anti-skid performance and overall strength of the road surface are improved. Warm mix ultra-thin overlay technology is a new road maintenance technology that combines warm mix asphalt mixture technology with ultra-thin overlay technology.

[0004] In order to adapt to the promotion and use of the "four new technologies" of low resource consumption, low carbon emissions, no waste disposal, and low resource consumption (asphalt, stone) road construction, 1-1.5cm warm-mixed ultra-thin overlay materials are increasingly used in maintenance and renovation. Warm-mixed ultra-thin overlay materials do not produce waste in pavement pre-maintenance and renovation and upgrading, and only require no milling and no roughening of old asphalt pavements and cement pavements. No milling and no waste generation protects the environment, which is more in line with the national green environmental protection policy, and is suitable for white-to-black cement pavements, asphalt pavement repair and pre-maintenance, and colored greenway construction and renovation maintenance. At the same time, no milling and no roughening of the original pavement ensures that the original old pavement structure strength is not damaged while repairing the functionality of the surface layer. Warm-mixed ultra-thin overlay technology can greatly improve the road performance and road surface function, which is conducive to the construction and maintenance needs of urban roads in the new era. This technology can comprehensively play the advantages of the two technologies, green and environmentally friendly, energy-saving and economical, simple construction process, and save later maintenance costs.

[0005] The combination of the smooth old road surface and the warm-mixed ultra-thin overlay requires a special waterproof adhesive layer material with high bonding strength and the ability to prevent rainwater from penetrating into the lower base. In particular, the application of warm-mixed ultra-thin overlay in the conversion of white cement pavement to black requires a special waterproof adhesive layer material with high permeability, high bonding force, but no wheel sticking (non-stick wheels prevent the sticky layer oil from being carried away by the material truck or paver, forming a blank strip), so that the 1-1.5cm warm-mixed ultra-thin overlay material can adhere firmly to the cement bonding surface. Domestic and foreign research results show that the overlay project does not pay enough attention to the setting of the waterproof layer, and generally only requires the setting of the bonding layer. Rainwater will still cause water damage to the overlay layer and the underlying asphalt pavement. Due to the existence of certain gaps and cracks in the asphalt surface layer, moisture will enter the pavement structure layer. If there is no waterproof layer in the overlay structure, rainwater will inevitably enter the overlay layer and the underlying original asphalt structure layer. Rainwater accumulates in the pavement structure layer for a long time. Under the action of vehicle load, a very unfavorable state is formed, which can easily lead to the destruction of the pavement structure layer under the combined action of water and load. A large number of asphalt pavement overlays.

[0006] The existing bonding layer materials generally use emulsified asphalt (ordinary emulsified asphalt and modified emulsified asphalt), and the dosage is generally 0.5-1kg / ㎡. Synchronous paving equipment is generally used (synchronous paving equipment is rare and expensive) to improve the demulsification efficiency and reduce the cooling of the ultra-thin layer asphalt mixture by moisture after demulsification. During the one-step paving construction process, the traditional emulsified bonding layer is easily taken away by the material truck and paving equipment, resulting in a local non-bonding layer, which is easy to cause local block removal and other diseases and hidden dangers. At present, the discharge temperature of the hot-mixed ultra-thin layer on the market is generally controlled at 175-185℃, and the synchronous paving rolling initial pressure temperature is generally required to be between 140-150℃. If asynchronous implementation requires waiting for demulsification and moisture after demulsification, it cannot be constructed in the low temperature seasons of spring, autumn and winter or in high-cold areas (ground temperature is below 10℃ or temperature is below zero), which limits the seasonality and openness of construction. The warm-mixed ultra-thin layer solves the openness and versatility of the surface layer during construction seasons (it can be constructed at ground temperatures above -2°C), but the bonding layer and waterproof layer combined above and below need to develop a new special waterproof bonding layer to match the warm-mixed ultra-thin layer. In general, the problems existing in the existing technology are as follows: (1) The emulsified asphalt demulsification construction requires a long waiting time and a large amount of spreading; (2) The adhesion strength is not enough, especially for the original asphalt and cement pavement without milling and roughening, the adhesion strength on the smooth bonding surface is insufficient and the durability is insufficient; (3) It is not conducive to ultra-thin construction when the pavement temperature is below 10°C. The water evaporates slowly after the emulsified asphalt is demulsified, and the water is easy to condense in low temperature seasons. These problems limit the seasonality and openness of the construction; (4) It is easy to stick to the wheels, which takes away the adhesive layer oil and easily causes the ultra-thin surface to delaminate and fall off; (5) Synchronous paving equipment is required, which has few equipment, high cost and poor construction convenience; (6) The amount of emulsified asphalt adhesive layer used is large. Summary of the invention

[0007] In view of the above-mentioned deficiencies in the prior art, the present invention provides a waterproof adhesive layer material suitable for warm-mix thin-layer overlay and a preparation method thereof, which is used to solve the problems of easy adhesion to wheels, large usage, long construction waiting time, seasonal construction and openness restrictions, insufficient adhesion strength, etc. The special waterproof adhesive layer material is not easily taken away by material trucks and paving equipment, has a low usage amount, can be stored for a long period of time, and has the advantages of good stability, good permeability, good adhesion, small seasonal construction restrictions, and no special equipment restrictions.

[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0009] The invention discloses a waterproof adhesive layer material suitable for warm-mix thin-layer covering. The adhesive layer material is prepared by using 8%-12% of mixed rubber powder, 3-4% of rock asphalt, 2-4% of silicon asphalt, 6-8% of intermediate, 1-4% of dispersant, 1.5-2.5% of flame retardant, 1-2% of stabilizer and 65-74.5% of solvent oil as raw materials through ball milling and colloid milling. The mixed rubber powder is a mixed powder composed of SBS rubber powder and SBR rubber powder in a mass ratio of 2-4:3-6. The intermediate is prepared by using 55% of tung oil, 5% of C9 resin, 5% of C5 resin, 30% of C10 liquid petroleum resin, 3% of acrylic acid and 2% of resin catalyst as raw materials through reaction in a reactor at 150-180°C for 8-12 hours.

[0010] The above-mentioned waterproof adhesive layer material suitable for warm-mix thin layer covering is preferably made by ball milling and mixing, in terms of mass percentage, 10% mixed rubber powder, 3% rock asphalt, 2% silicone asphalt, 6% intermediate, 1% dispersant, 1.5% flame retardant, 2% stabilizer and 74.5% solvent oil as raw materials.

[0011] The above waterproof adhesive layer material suitable for warm-mix thin-layer overlay, styrene-butadiene rubber (SBR) is also called polystyrene butadiene copolymer. Its physical structure performance, processing performance and product performance are close to natural rubber. Some properties such as wear resistance, heat resistance, aging resistance and vulcanization speed are better than natural rubber, and it can be used with natural rubber and various synthetic rubbers. Styrene-butadiene-styrene block copolymer (SBS) is a block copolymer form of styrene-butadiene rubber produced by anionic block copolymerization. S represents styrene, B represents butadiene, and the two ends of the polymer are styrene polymer segments, and the middle is a butadiene polymer segment, forming an ABA-type triblock copolymer. SBS rubber usually refers to SBS after hydrogenation treatment. The double bonds in the polybutadiene block are eliminated by hydrogenation treatment, so that SBS rubber has good antioxidant ability. As the most widely used modifier at present, SBS has excellent elastic recovery performance and very good viscoelasticity. At the same time, its excellent flexibility can improve the problem of insufficient viscosity and toughness of SBR and increase adhesion to aggregates. In the present invention, the rubber mixed powder composed of SBS rubber powder and SBR rubber powder preferably has a particle size of 100-300 mesh. The mixed rubber powder can be produced by conventional methods in the art. The mixed rubber powder is preferably prepared by the following method: SBS rubber and SBR rubber are uniformly mixed in a mass ratio of 2-4:3-6 and are kneaded into sheets by an open mill, and then the pieces are cut into pieces by a slicer, and the pieces are ground into a powdery material of 100-300 mesh by a low-temperature liquid nitrogen powder mill, so as to obtain the mixed rubber powder. Using liquid nitrogen as a grinding medium can achieve the comprehensive effects of low-temperature crushing, explosion-proof and anti-oxidation of materials.

[0012] The above waterproof adhesive layer material suitable for warm-mix thin-layer overlay, the function of the dispersant is to promote the uniform dispersion of material particles in the medium to form a stable suspension. The dispersant can be a commonly used dispersant in the art without special restrictions, preferably a polycarboxylate sodium salt type dispersant, which has an excellent dispersing effect on fillers with poor fluidity.

[0013] The above-mentioned waterproof adhesive layer material suitable for warm-mix thin-layer covering, the flame retardant is a special chemical additive used to improve the combustion performance of combustible and flammable materials. In the present invention, the flame retardant can be a conventional flame retardant in the field, preferably but not limited to a halogen-free flame retardant, and more preferably a halogen-free phosphorus flame retardant.

[0014] The above-mentioned waterproof adhesive layer material is suitable for warm-mix thin-layer covering. The stabilizer is mainly used to stabilize the material. In this invention, the stabilizer can adopt conventional stabilizers in the field, and preferably adopts but is not limited to hindered amine light stabilizers.

[0015] The above waterproof adhesive layer material suitable for warm-mix thin-layer overlay has a flash point, also known as the flash point, which is the lowest temperature point at which a flash fire occurs and burns immediately when the oil and the outside air form a mixed gas and come into contact with the flame. The solvent oil preferably uses a high flash point solvent oil with a flash point greater than 85.

[0016] The above-mentioned waterproof adhesive layer material suitable for warm-mix thin-layer overlay, tung oil is an excellent drying vegetable oil, and the present invention adopts pure tung oil. C9 resin (C9 petroleum resin) is a thermoplastic resin prepared by polymerizing the C9 fraction, a by-product of the cracking ethylene production unit, in the presence of a catalyst, or copolymerizing it with aldehydes, aromatic hydrocarbons, and terpene compounds. C5 (petroleum) resin, also known as C5 resin and aliphatic hydrocarbon resin, has good tackifying properties, heat resistance, stability, water resistance, acid and alkali resistance, and the tackifying effect is generally better than C9 resin. It has good compatibility with phenolic resin, terpene resin, coumarone resin, natural rubber, synthetic rubber, etc., especially with styrene-butadiene rubber (SBR), and has excellent compatibility. The resin catalyst can be a conventional resin catalyst in the art, and there is no special restriction. In the present invention, the resin catalyst adopts the reactant YKCHWD-1, which is a bead formed by suspension copolymerization of styrene and divinylbenzene under the action of a special pore-forming agent, and then a high molecular polymer with a macroporous network and sulfonic acid groups is obtained by sulfonation reaction.

[0017] The present invention also provides a method for preparing a waterproof adhesive layer material suitable for a warm-mix thin-layer overlay, comprising the following steps:

[0018] S1. Weigh the mixed rubber powder, rock asphalt, silicon asphalt, intermediate, dispersant, flame retardant, stabilizer and solvent oil in proportion and add them into a ball mill for ball milling, so that each raw material is dissolved or dispersed in the ball milling state to obtain a primary slurry. The ball milling is carried out at room temperature and normal pressure until each raw material is dissolved or dispersed in the ball milling state;

[0019] S2. The primary slurry is sent to the hopper of the colloid mill and ground by the colloid mill to obtain a waterproof bonding layer material suitable for warm-mix thin-layer covering.

[0020] In the above method for preparing a waterproof adhesive layer material suitable for a warm-mix thin-layer overlay, in step S1, the purpose of ball milling is to dissolve or disperse each raw material in the ball milling state, so the ball milling time can be set according to the conventional method. Usually, the ball milling time of 0.5-1 hour can meet the requirements, and the ball milling speed is preferably 4-6 rpm. In step S2, the colloid milling time is preferably 1 to 3 hours, and the colloid milling speed is 1200 to 1600 rpm.

[0021] The above-mentioned preparation method of the waterproof adhesive layer material suitable for warm-mix thin layer covering, when the waterproof adhesive layer material is prepared in step S2, the product usually needs to be canned or shipped, so the preparation method also includes the following steps: step S3, finished product filling process 200kg / barrel or spreader tank truck shipment.

[0022] The preparation method of the waterproof adhesive layer material suitable for warm-mixed thin-layer overlay is a rubber mixed powder composed of SBS rubber powder and SBR rubber powder, and its particle size is preferably 100-300 mesh. The mixed rubber powder can be produced and prepared by conventional methods in the art. The mixed rubber powder is preferably prepared by the following method: SBS rubber and SBR rubber are evenly mixed in a mass ratio of 2 to 4:3 to 6 and are kneaded into sheets using an open mill, and then the pieces are cut into pieces using a slicer, and the pieces are ground into a powdery material of 100-300 mesh by a low-temperature liquid nitrogen powder mill, so as to obtain a mixed rubber powder. Using liquid nitrogen as a grinding medium can achieve the comprehensive effects of low-temperature crushing, explosion-proof and anti-oxidation of materials.

[0023] The above-mentioned preparation method of waterproof adhesive layer material suitable for warm-mixed thin-layer overlay, colloid mill and ball mill are both grinding and crushing machine series. The ball mill grinds and disperses liquid and solid phase materials, and has special effects on materials that are easy to return to coarseness and thickening. The colloid mill is a wet material micro-processing machine that can crush, emulsify, homogenize and mix various semi-fluid and emulsion substances. Its principle is that through the relative movement of rotor grinding teeth and stator grinding teeth of different geometric shapes under high-speed rotation, the processed materials are subjected to strong shear force, friction force and high-frequency vibration when passing through its adjustable annular gap under the action of composite forces such as self-gravity and centrifugal force, so as to achieve the purpose of dispersion, crushing, emulsification, homogenization and mixing. The core component stator and rotor are equipped with three-level grinding areas, the first level is the coarse grinding area, the second level is the fine grinding area, and the third level is the ultra-fine grinding area. There are various grinding teeth designed according to the different material properties and processing requirements. In the present invention, the raw materials are firstly fully dissolved and dispersed by ball milling, and the mixed materials after ball milling are then subjected to high-speed shearing, grinding and crushing by a colloid mill, thereby producing the effects of liquid material molecular chain breaking, particle crushing, liquid particle tearing and the like, so that the materials can be fully dispersed, crushed, emulsified, homogenized and refined.

[0024] Compared with the prior art, the waterproof adhesive layer material suitable for warm-mix thin-layer overlay and the preparation method thereof provided by the present invention have the following beneficial effects:

[0025] (1) Low usage: 0.3-0.4kg / ㎡ for converting white mud road surface to black, 0.2-0.3kg / ㎡ for overlaying asphalt road surface. The usage of existing emulsified asphalt (ordinary emulsified asphalt and modified emulsified asphalt) is generally 0.5-1kg / ㎡, so the usage is relatively lower, which can effectively reduce the road maintenance cost.

[0026] (2) Low spray viscosity and non-stick wheels: The waterproof adhesive layer material has low spray viscosity, is easy to construct and spray, and is not easily carried away by material trucks and paving equipment, effectively solving problems and hidden dangers such as local lack of adhesive layer and local debonding. At the same time, the non-stick wheel effect makes the operation of paving equipment and material trucks more convenient and worry-free.

[0027] (3) Long-term turnover and storage: No segregation, good stability, no demulsification, and can be stored for a long period of more than 2 years.

[0028] (4) High adhesion strength: The bonding strength of the waterproof adhesive layer material is above 1MPa. Especially when it is used to convert white to black, it does not require milling or roughening of the original asphalt and cement pavement. It has high adhesion strength on the smooth bonding surface, sufficient durability, and has a forward-looking advantage.

[0029] (5) The preparation method is simple: the waterproof adhesive layer material can be obtained by grinding with a ball mill or a colloid mill. The steps are simple, the operability is strong, and it is easy to mass-produce industrially.

[0030] (6) In general, the waterproof bonding layer material has good permeability, good adhesion, little seasonal construction restrictions, no special equipment restrictions, and can be ultra-thinly constructed at road surface temperatures below 10°C. It can effectively solve the problems of slow evaporation of water after emulsified asphalt demulsification and easy condensation of water in low temperature seasons, breaking the restrictions of seasonal construction and openness. There is no need to mill or roughen the original road surface, which will damage the structural strength of the original road surface. Paving is simpler, faster, more efficient, low-carbon, and environmentally friendly. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention is further described below in conjunction with embodiments.

[0032] The mixed rubber powder used in the following examples has a particle size of 100-300 meshes and is prepared by the following method: SBS rubber and SBR rubber are uniformly mixed in a mass ratio of 2-4:3-6 and kneaded into sheets using an open mixer, and then cut into pieces using a slicer, and the pieces are ground into a powdery material of 100-300 meshes using a low-temperature liquid nitrogen grinder to obtain the mixed rubber powder.

[0033] In the following examples, the dispersant is SN-5040, the flame retardant is flame retardant-601, the stabilizer is stabilizer 5050, the solvent oil is S-1800, 120#, and the resin catalyst is YKCHWD-1.

[0034] Example 1

[0035] The present embodiment provides a waterproof adhesive layer material suitable for warm-mix thin-layer covering, which is made of 10% mixed rubber powder, 3% rock asphalt, 2% silicon asphalt, 6% intermediate, 1% dispersant, 1.5% flame retardant, 2% stabilizer, and 74.5% solvent oil as raw materials, which are processed by ball milling and colloid milling in sequence. The particle size of the mixed rubber powder is 100 mesh, and it is a mixed powder composed of SBS rubber powder and SBR rubber powder in a mass ratio of 2:3. The intermediate is made of 55% tung oil, 5% C9 resin, 5% C5 resin, 30% C10 liquid petroleum resin, 3% acrylic acid, and 2% resin catalyst as raw materials, which are reacted in a reactor at 160°C for 10 hours. It is prepared by the following steps:

[0036] S1. Weigh the mixed rubber powder, rock asphalt, silicon asphalt, intermediate, dispersant, flame retardant, stabilizer and solvent oil in proportion and add them into a ball mill for ball milling. The ball milling speed is 4 rad / min and the ball milling time is 0.5 h. All the raw materials are completely dissolved or dispersed in the ball milling state to obtain a primary slurry. The ball milling is carried out at room temperature and normal pressure until all the raw materials are completely dissolved or dispersed in the ball milling state.

[0037] S2, sending the primary slurry to the hopper of the colloid mill and grinding it through the colloid mill for 1 hour, the rotation speed of the colloid mill is 1500 rpm, and obtaining a waterproof bonding layer material suitable for warm-mix thin layer overlay;

[0038] S3. Finished product filling process: 200kg / barrel or shipped by spreader tank truck.

[0039] Embodiments 2 to 5

[0040] The difference between Examples 2 to 5 and Example 1 is only that the addition ratio of each raw material is different. Please refer to Table 1 for the specific addition ratio.

[0041] Table 1 Preparation of waterproof bonding layer materials suitable for warm mix thin layer overlay with different raw material ratios

[0042]

[0043] Embodiments 6 to 8

[0044] The only difference between Examples 6 to 8 and Example 1 is that the mixing ratio of SBS rubber powder and SBR rubber powder in the mixed rubber powder is different and the particle size of the mixed rubber powder is different. Please refer to Table 2 for specific parameters.

[0045] Table 3 Preparation of waterproof bonding layer materials suitable for warm-mixed thin-layer overlays by different mixed rubber powder particle sizes and mixing ratios

[0046]

[0047]

[0048] The performance of the waterproof adhesive layer material suitable for warm-mix thin-layer overlay prepared in Example 1 was tested, and the specific testing methods and standards are shown in Table 3.

[0049] Table 3 Testing methods and standards for waterproof adhesive layer materials

[0050]

[0051] After testing, the waterproof adhesive layer material suitable for warm-mixed thin-layer covering prepared in Example 2 (white to black) has a viscosity of 75 mPa·s, a storage stability of 0.3, a sieve residue of 0.05, and a bonding strength of 1.08 Mpa.

[0052] Application Examples

[0053] This application example adopts Example 1, which is suitable for a waterproof adhesive layer material for a warm-mix thin layer cover. The construction object is the "black to black" project of Shuangnan Avenue in Shuangliu District, Chengdu City, Sichuan Province. The construction area is 230,000 square meters, and the usage is (0.3) kg / ㎡.

[0054] This application example adopts Example 2, which is a waterproof adhesive layer material suitable for warm-mix thin-layer covering, and takes the "white to black" project of Wujiaba South Street, Shuangliu District, Chengdu City, Sichuan Province as the construction object, with a construction area of ​​30,000 square meters and a usage of 0.4kg / m2.

[0055] Construction, transportation and storage:

[0056] 1. Preparation of construction tools: Mixing bucket, spraying machine or special bristle brush should be prepared before construction.

[0057] 2. Base requirements: The concrete strength should reach the design grade, and there should be no loose slurry, peeling, hollowing and severe cracking on the surface. The surface flatness should meet the requirements of highway specifications, and the base should be clean, dry and free of water.

[0058] 4. Base treatment: The base surface must not have dust, floating dust, impurities, oil stains, etc. Before making the waterproof layer, the surface can be cleaned with an air compressor, water purification, degreasing agent, etc. If there are hardened debris such as concrete and mortar, they should be polished off.

[0059] Waterproof layer construction steps: (taking three coatings as an example, the waterproof bonding layer material is referred to as coating below)

[0060] 1) The barreled paint product should be stirred evenly before painting.

[0061] 2) Before painting a large area, use a small brush to apply two coats of paint to the leaking area, apply waterproof paint three times to the inner corners, and then apply the first coat of paint to the large area.

[0062] 3) After the first coat of paint is completely dry, you can apply the second coat of paint.

[0063] 4) Apply the third coat of paint after the second coat of paint has dried on the surface.

[0064] 5) Paint consumption: 0.3-0.4kg / ㎡.

[0065] 6) The construction temperature should be between 0 and 35 degrees Celsius. Construction should not be carried out on rainy days or during freezing periods.

[0066] 7) Packaging The product is packed in iron barrels with lids, each barrel weighing 200kg.

[0067] 8) Transportation: This product is non-toxic and non-flammable and can be transported by general means.

[0068] 9) Storage: The product has a shelf life of more than 2 years and should be stored in a warehouse above 0 degrees Celsius. It should be kept away from direct sunlight in summer.

[0069] To sum up, the construction process of the waterproof bonding layer is simple, the waterproof layer is firmly bonded to the base layer and the upper asphalt concrete, the usage is low, the drying is fast, the construction period is short, it is not easily carried away by material trucks and paving equipment, the usage is low, and it can be stored for a long period of time. It has the advantages of good stability, good permeability, good adhesion, little seasonal construction restrictions, and no special equipment restrictions.

[0070] The above is only an embodiment of the present invention. The common sense such as the known specific structure and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field are aware of all the common technical knowledge in the technical field of the invention before the application date or priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement the scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for the ordinary technicians in the relevant field to implement this application. It should be pointed out that for the technicians in this field, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A waterproof adhesive layer material suitable for warm-mix thin layer overlay, characterized in that: Measured by mass percentage, the bonding layer material is prepared by using 8%-12% of mixed rubber powder, 3-4% of rock asphalt, 2-4% of silicon asphalt, 6-8% of intermediate, 1-4% of dispersant, 1.5-2.5% of flame retardant, 1-2% of stabilizer and 65-74.5% of solvent oil as raw materials, and grinding them in sequence through ball milling and colloid milling. The mixed rubber powder is a mixed powder composed of SBS rubber powder and SBR rubber powder in a mass ratio of 2-4:3-6. The intermediate is prepared by using 55% of tung oil, 5% of C9 resin, 5% of C5 resin, 30% of C10 liquid petroleum resin, 3% of acrylic acid and 2% of resin catalyst as raw materials, and reacting in a reactor at a temperature of 150-180°C for 8-12 hours.

2. The waterproof adhesive layer material suitable for warm-mix thin layer overlay according to claim 1, characterized in that: Calculated by mass percentage, the bonding layer material is made by ball milling and mixing with 10% mixed rubber powder, 3% rock asphalt, 2% silicon asphalt, 6% intermediate, 1% dispersant, 1.5% flame retardant, 2% stabilizer and 74.5% solvent oil.

3. The waterproof adhesive layer material suitable for warm-mix thin layer overlay according to claim 1, characterized in that: Therefore, the particle size of the mixed rubber powder is 100-300 mesh.

4. The waterproof adhesive layer material suitable for warm mix thin layer overlay according to claim 3, characterized in that: The mixed rubber powder is prepared by the following method: SBS rubber and SBR rubber are uniformly mixed in a mass ratio of 2-4:3-6, and are kneaded into sheets by an open mill, and then the pieces are cut into pieces by a slicer, and the pieces are ground into powdery materials of 100-300 meshes by a low-temperature liquid nitrogen powder mill, so as to obtain the mixed rubber powder.

5. The waterproof adhesive layer material suitable for warm-mix thin layer overlay according to claim 1, characterized in that: The dispersant is a polycarboxylate sodium salt type dispersant.

6. The waterproof adhesive layer material suitable for warm mix thin layer overlay according to claim 1, characterized in that: The flame retardant is a halogen-free flame retardant.

7. The waterproof adhesive layer material suitable for warm-mix thin layer overlay according to claim 1, characterized in that: The stabilizer is a hindered amine light stabilizer.

8. The waterproof adhesive layer material suitable for warm mix thin layer overlay according to claim 1, characterized in that: The solvent oil is a high flash point solvent oil with a flash point greater than 85.

9. A method for preparing a waterproof adhesive layer material suitable for warm-mix thin-layer overlay as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: S1. Weigh the mixed rubber powder, rock asphalt, silicon asphalt, intermediate, dispersant, flame retardant, stabilizer and solvent oil in proportion and add them into a ball mill for ball milling, so that each raw material is dissolved or dispersed in the ball milling state to obtain a primary slurry. The ball milling is carried out at room temperature and normal pressure until each raw material is dissolved and dispersed in the ball milling state; S2. The primary slurry is sent to the hopper of the colloid mill for dispersion and grinding by the colloid mill to obtain a waterproof bonding layer material suitable for warm-mix thin-layer covering.

10. The method for preparing a waterproof adhesive layer material suitable for warm-mix thin-layer overlay according to claim 9, characterized in that: The mixed rubber powder is prepared by the following method: SBS rubber and SBR rubber are uniformly mixed in a mass ratio of 2-4:3-6, and are kneaded into sheets by an open mill, and then the pieces are cut into pieces by a slicer, and the pieces are ground into powdery materials of 100-300 meshes by a low-temperature liquid nitrogen powder mill, so as to obtain the mixed rubber powder.

Citation Information

Patent Citations

  • Modified asphalt composition for warm-mixed thin overlay and preparation method of modified asphalt composition

    CN111286207A

  • Pavement structure adopting warm mixing ultrathin layer overlay and construction method of pavement structure