A method for in-situ synthesis of interpenetrating organic network and silicon network composite passivation film

Through the in-situ synthesis of interpenetrating organic network-silicon network composite film, the problems of chromate carcinogenicity and insufficient corrosion resistance of silane films are solved, cost reduction and performance improvement are achieved, and are suitable for passivation treatment of carbon steel.

CN115652295BInactive Publication Date: 2024-11-26INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211363478.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-02
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing passivation technology, the use of chromate has carcinogenic risks and environmental threats, and the corrosion resistance and cost problems of the silane passivation film have not been met.

Method used

Using the method of synthesizing interpenetrating organic network-silicon network composite passivation film in situ, the silicon source and organic material form a composite passivation liquid under the action of specific solvents and initiators, soak and dry carbon steel to obtain interpenetration. Organic network-silicon network composite film reduces costs and improves corrosion resistance.

Benefits of technology

It effectively reduces the cost of silane passivation, improves the corrosion resistance and ductility of the film, reduces cracking during the preparation process, and improves the stability of the passivation liquid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003922880810000101
    Figure BDA0003922880810000101
  • Figure BDA0003922880810000111
    Figure BDA0003922880810000111
Patent Text Reader

Abstract

The present invention provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the synthesis method comprising: mixing a silicon source with a first solvent to obtain a first solution; mixing an organic material with a second solvent, adding an initiator to obtain a second solution; mixing the first solution with the second solution, adding a terminator to obtain a passivation solution; soaking carbon steel in the passivation solution, and drying to obtain an interpenetrating organic network-silicon network composite passivation film. The method reduces the cost of silane passivation, improves the corrosion resistance of the silane passivation film, and also improves the ductility of the silane film, reducing the phenomenon of cracking during preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of passivation treatment, relates to a method for synthesizing a passivation film, and in particular to a method for in-situ synthesizing an interpenetrating organic network-silicon network composite passivation film. Background Art

[0002] Surface passivation of carbon steel can greatly increase the service life of carbon steel and save a lot of money every year. At present, chromate is commonly used to passivate carbon steel, but because chromate contains hexavalent chromium, which is a carcinogen and poses a serious threat to human health and the environment, hexavalent chromium passivation technology has been restricted or even abandoned by countries around the world. At present, many studies have used silane passivation to treat carbon steel, but the corrosion resistance of the resulting film layer is still not satisfactory, and the high price is also one of the main factors restricting its development.

[0003] Polymer interpenetrating networks, especially organic / inorganic polymer interpenetrating network materials, partially overcome the performance defects of single materials and traditional composite materials, so that the materials have both the advantages of inorganic materials (such as rigidity, high thermal stability) and the advantages of polymer materials (such as elasticity, dielectric properties, ductility and processability, etc.), and produce additional performance improvements due to the formation of an interpenetrating network structure between the two components. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, which reduces the cost of silane passivation, improves the corrosion resistance of the silane passivation film, and also improves the ductility of the silane film, reducing the cracking phenomenon during preparation.

[0005] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the synthesis method comprising:

[0007] Mixing a silicon source with a first solvent to obtain a first solution;

[0008] Mixing the organic material with the second solvent and adding an initiator to obtain a second solution;

[0009] The first solution and the second solution are mixed, and a terminator is added to obtain a passivation solution;

[0010] The carbon steel is immersed in the passivation solution and dried to obtain an interpenetrating organic network-silicon network composite passivation film.

[0011] In the present invention, an organic network and a silicon network are compounded when preparing a passivation film to form an organic network-silicon network composite passivation film. The introduction of an organic network structure reduces the preparation cost of the silane film on the one hand, and improves the corrosion resistance of the silane film on the other hand. At the same time, due to the addition of organic matter, the ductility of the silane film and the stability of the passivation solution are improved, and the phenomenon of long-term stratification is alleviated. The in-situ synthesis method is adopted to simplify the production steps.

[0012] As a preferred technical solution of the present invention, the silicon source includes sodium silicate and / or ethyl orthosilicate.

[0013] Preferably, the first solvent comprises an aqueous solution of alcohol, and the mass ratio of the alcohol to water is 3-7:7-3, 3.5:6.5, 4:6, 4.5:5.5, 5:4, 5.5:4.5, 6:4 or 6.5:3.5, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] Preferably, the alcohol comprises any one of methanol, ethanol or isopropanol or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of methanol and ethanol, a combination of ethanol and isopropanol, a combination of isopropanol and methanol, or a combination of methanol, ethanol and isopropanol, etc.

[0015] Preferably, the mass ratio of the silicon source to the first solvent is 1:4-8, such as 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7 or 1:7.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] As a preferred technical solution of the present invention, the silicon source and the first solvent are mixed under stirring.

[0017] Preferably, the stirring rate is 300-800 rpm, such as 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm or 750 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the stirring time is 1 to 3 h, such as 1.2 h, 1.5 h, 1.8 h, 2 h, 2.2 h, 2.5 h or 2.8 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] As a preferred technical solution of the present invention, the organic material includes any one of cellulose, polyvinyl alcohol, alginic acid, phytic acid or polyethylene glycol, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of cellulose and polyvinyl alcohol, a combination of polyvinyl alcohol and alginic acid, a combination of alginic acid and phytic acid, a combination of phytic acid and polyethylene glycol, a combination of polyethylene glycol and cellulose, or a combination of cellulose, polyvinyl alcohol and alginic acid, etc.

[0020] Preferably, the second solvent comprises water.

[0021] Preferably, the mass ratio of the organic material to the silicon source is 1 to 2:1, such as 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1 or 1.9:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the mass ratio of the organic material to the second solvent is 1:3-5, such as 1:3.2, 1:3.5, 1:3.8, 1:4, 1:4.2, 1:4.5 or 1:4.8, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] As a preferred technical solution of the present invention, the initiator includes any one of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, 1-diphenyl-2-trinitrophenylhydrazine, toluidine, N-nitrodiphenylamine, benzoyl peroxide, tert-butyl benzoyl peroxide or methyl ethyl ketone peroxide, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of azobisisobutyronitrile and azobisisoheptanenitrile, a combination of azobisisoheptanenitrile and dimethyl azobisisobutyrate, a combination of dimethyl azobisisobutyrate and 1-diphenyl-2-trinitrophenylhydrazine, a combination of 1-diphenyl-2-trinitrophenylhydrazine and toluidine, a combination of toluidine and N-nitrodiphenylamine, a combination of N-nitrodiphenylamine and benzoyl peroxide, a combination of benzoyl peroxide and tert-butyl benzoyl peroxide, or a combination of tert-butyl benzoyl peroxide and methyl ethyl ketone peroxide, etc.

[0024] Preferably, the mass ratio of the organic material to the initiator is 1:0.001-0.01, such as 1:0.002, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007, 1:0.008 or 1:0.009, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] As a preferred technical solution of the present invention, stirring is performed after the initiator is added.

[0026] Preferably, the stirring rate is 300-800 rpm, such as 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm or 750 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the stirring temperature is 50-80°C, such as 55°C, 60°C, 65°C, 70°C or 75°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] As a preferred technical solution of the present invention, the terminator includes any one of hydroquinone, p-tert-butylcatechol, sodium dimethyldithiocarbamate, sodium polysulfide or sodium nitrite, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of hydroquinone and p-tert-butylcatechol, a combination of p-tert-butylcatechol and sodium dimethyldithiocarbamate, a combination of sodium dimethyldithiocarbamate and sodium polysulfide, a combination of sodium polysulfide and sodium nitrite, or a combination of sodium nitrite and hydroquinone.

[0029] Preferably, the mass ratio of the organic material to the terminator is 1:0.001-0.01, such as 1:0.002, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007, 1:0.008 or 1:0.009, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] In the present invention, the function of the terminator is to block the polymerization reaction of the organic material to prevent the over-polymerization from causing solidification and loss of usability.

[0031] In the present invention, after the first solution and the second solution are mixed, a terminator and a silane coupling agent can be added at the same time. The terminator can prevent excessive polymerization of organic matter, and the silane coupling agent can increase the bonding degree between the organic network and the inorganic network in the form of "bridging".

[0032] As a preferred technical solution of the present invention, stirring is performed after the terminator is added.

[0033] Preferably, the stirring rate is 300-800 rpm, such as 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm or 750 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the stirring time is 1 to 3 h, such as 1.2 h, 1.5 h, 1.8 h, 2 h, 2.2 h, 2.5 h or 2.8 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] As a preferred technical solution of the present invention, the soaking time is 1 to 10 minutes, such as 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes or 9 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] As a preferred technical solution of the present invention, the drying temperature is 100-150°C, such as 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C or 145°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the drying time is 10 to 60 min, such as 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min or 55 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Compared with the prior art, the present invention has at least the following beneficial effects:

[0039] (1) The present invention provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, which reduces the cost of silane passivation and improves the corrosion resistance of the silane passivation film;

[0040] (2) The present invention provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, which improves the ductility of the silane film, reduces cracking during preparation, and improves the stability of the passivation solution. DETAILED DESCRIPTION

[0041] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0042] Example 1

[0043] This embodiment provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the method comprising:

[0044] 20 g of tetraethyl orthosilicate was added to 80 g of an ethanol-water mixed solution having an alcohol-water ratio of 3:7, and stirred at 500 r / min for 2 h to obtain a first solution;

[0045] 20 g of polyvinyl alcohol was added to 80 g of water, and then 0.1 g of azobisisobutyronitrile and 0.1 g of 1-diphenyl-2-trinitrophenylhydrazine were added, and stirred at 60° C. and 500 r / min until slightly viscous to obtain a second solution 2;

[0046] Pour the first solution into the second solution, mix well, add 0.1 g of hydroquinone and silane coupling agent, continue stirring at 500 r / min for 1 h, and obtain a passivation solution;

[0047] The carbon steel was immersed in the passivation solution for 2 minutes, taken out and dried at 120°C for 30 minutes to obtain an interpenetrating organic network-silicon network composite passivation film.

[0048] Example 2

[0049] This embodiment provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the method comprising:

[0050] 20 g of tetraethyl orthosilicate was added to 80 g of an ethanol-water mixed solution having an alcohol-water ratio of 5:5, and stirred at 500 r / min for 2 h to obtain a first solution;

[0051] 20 g of cellulose was added to 80 g of water, and then 0.1 g of dimethyl azobisisobutyrate and 0.1 g of 1-diphenyl-2-trinitrophenylhydrazine were added, and stirred at 60° C. and 500 r / min until slightly viscous to obtain a second solution;

[0052] Pour the first solution into the second solution, mix well, add 0.1 g of p-tert-butylcatechol and silane coupling agent, continue stirring at 500 r / min for 1 hour, and obtain a passivation solution;

[0053] The carbon steel was immersed in the passivation solution for 2 minutes, taken out and dried at 120°C for 30 minutes to obtain an interpenetrating organic network-silicon network composite passivation film.

[0054] Example 3

[0055] This embodiment provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the method comprising:

[0056] 20 g of sodium silicate was added to 80 g of an ethanol-water mixed solution having an alcohol-water ratio of 7:3, and stirred at 500 r / min for 2 h to obtain a first solution;

[0057] Add 20g of polyvinyl alcohol to 80g of water, then add 0.1g of N-nitrodiphenylamine and 0.1g of benzoyl peroxide, stir at 60°C and 500r / min until slightly viscous, to obtain a second solution;

[0058] Pour the first solution into the second solution, mix well, add 0.1 g of sodium dimethyldithiocarbamate and silane coupling agent, continue stirring at 500 r / min for 1 h to obtain a passivation solution;

[0059] The carbon steel was immersed in the passivation solution for 2 minutes, taken out and dried at 120°C for 20 minutes to obtain an interpenetrating organic network-silicon network composite passivation film.

[0060] Example 4

[0061] This embodiment provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the method comprising:

[0062] 20 g of sodium silicate was added to 80 g of an ethanol-water mixed solution having an alcohol-water ratio of 7:3, and stirred at 500 r / min for 2 h to obtain a first solution;

[0063] 20 g of polyethylene glycol was added to 80 g of water, and then 0.1 g of N-nitrodiphenylamine and 0.1 g of benzoyl peroxide were added, and stirred at 60° C. and 500 r / min until slightly viscous to obtain a second solution;

[0064] Pour the first solution into the second solution, mix well, add 0.1 g of sodium dimethyldithiocarbamate and silane coupling agent, continue stirring at 500 r / min for 1 h to obtain a passivation solution;

[0065] The carbon steel was immersed in the passivation solution for 2 minutes, taken out and dried at 120°C for 20 minutes to obtain an interpenetrating organic network-silicon network composite passivation film.

[0066] Comparative Example 1

[0067] This comparative example provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the method comprising:

[0068] 20 g of tetraethyl orthosilicate was added to 80 g of an ethanol-water mixed solution having an alcohol-water ratio of 3:7, and stirred at 500 r / min for 2 h to obtain a first solution;

[0069] Add 20g of polyvinyl alcohol to 80g of water, then add 0.1g of N-nitrodiphenylamine and 0.1g of benzoyl peroxide, stir at 60°C and 500r / min until slightly viscous, to obtain a second solution;

[0070] Pour the first solution into the second solution and add the silane coupling agent, mix well, continue stirring at 500 r / min for 1 hour to obtain a passivation solution;

[0071] The carbon steel was immersed in the passivation solution for 2 minutes, taken out and dried at 120°C for 20 minutes to obtain an interpenetrating organic network-silicon network composite passivation film.

[0072] Comparative Example 2

[0073] This comparative example provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the method comprising:

[0074] 20 g of tetraethyl orthosilicate was added to 80 g of an ethanol-water mixed solution having an alcohol-water ratio of 3:7, and stirred at 500 r / min for 2 h to obtain a first solution 1;

[0075] 20 g of cellulose was added into 80 g of water, and stirred at 60°C and 500 r / min to obtain a second solution;

[0076] Pour the first solution into the second solution, mix well, add 0.1 g of sodium dimethyldithiocarbamate and silane coupling agent, continue stirring at 500 r / min for 1 h, and obtain a passivation solution;

[0077] The carbon steel was immersed in the passivation solution for 2 minutes, taken out and dried at 120°C for 20 minutes to obtain an interpenetrating organic network-silicon network composite passivation film.

[0078] Comparative Example 3

[0079] This comparative example provides a method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film, the method comprising:

[0080] 10 g of sodium silicate was added to 80 g of an ethanol-water mixed solution having an alcohol-water ratio of 3:7, and stirred at 500 r / min for 2 h to obtain a first solution;

[0081] 20 g of alginic acid was added into 80 g of water, and stirred at 60°C and 500 r / min to obtain a second solution;

[0082] Pour the first solution into the second solution, mix well, add 0.1 g of sodium dimethyldithiocarbamate and silane coupling agent, continue stirring at 500 r / min for 1 h to obtain a passivation solution;

[0083] The carbon steel was immersed in the passivation solution for 2 minutes, taken out and dried at 120°C for 20 minutes to obtain an interpenetrating organic network-silicon network composite passivation film.

[0084] Comparative Example 4

[0085] In this comparative example, except that the carbon steel is directly immersed in the first solution, other conditions are the same as those of Example 1.

[0086] Comparative Example 5

[0087] In this comparative example, except that the carbon steel is directly immersed in the second solution, other conditions are the same as those of Example 1.

[0088] The passivation films prepared in Examples 1-4 and Comparative Examples 1-5 were subjected to a salt spray test, and the storage stability of the passivation solution was tested. The results are shown in Table 1.

[0089] The stability test method of the passivation solution is: static method. Use a 100mL measuring cylinder to take 50mL of the passivation solution and let it stand. When any of the following three conditions is met: the stratification volume is greater than 5mL, the precipitation volume is greater than 5mL, and the viscosity rises to the point where a film cannot be formed, it is considered to have lost stability.

[0090] The test method for the film layer bonding performance is: the bonding strength of the coating is tested according to GB / T 13936-2014 "Test method for tensile shear strength of bonding between vulcanized rubber and metal". If the bonding strength is greater than 2MPa, it is considered to be good, otherwise it is considered to be low.

[0091] The film uniformity test method is: use a portable thickness gauge, and the film is uniform if the difference between the thickest and thinnest parts is within 1mm and there are no obvious bubbles or depressions.

[0092] The corrosion resistance test method is: at 25°C, pH = 7, 3.5% sodium chloride solution, use a salt spray test machine to perform corrosion tests, and the time when obvious overall corrosion, filiform corrosion, crevice corrosion or pitting corrosion occurs is used as the standard for judging corrosion resistance.

[0093] Table 1

[0094]

[0095]

[0096] In Comparative Example 1, no terminator was added, resulting in excessive polymerization of the organic phase, a rapid increase in the overall viscosity, a decrease in the stability of the passivation solution, an increase in the difficulty of film formation, and a decrease in corrosion resistance.

[0097] In Comparative Example 2, no initiator was added, resulting in no polymerization of the organic phase, low overall viscosity, difficulty in film formation, and easy introduction of bubbles and depressions, resulting in uneven film layers, difficulty in controlling thickness, and decreased corrosion resistance.

[0098] In Comparative Example 3, no initiator was added and the sodium silicate content was low, resulting in less silane inorganic network formed, poor film-forming performance, low bonding strength, and decreased corrosion resistance.

[0099] The applicant declares that the present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for in-situ synthesis of an interpenetrating organic network-silicon network composite passivation film on a carbon steel surface, characterized in that: The synthesis method comprises: Mixing a silicon source with a first solvent to obtain a first solution; Mixing the organic material with the second solvent and adding an initiator to obtain a second solution; The organic material comprises any one of cellulose, alginic acid, phytic acid or polyethylene glycol, or a combination of at least two thereof; The initiator includes any one of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, 1-diphenyl-2-trinitrophenylhydrazine, toluidine, N-nitrodiphenylamine, benzoyl peroxide, tert-butyl benzoyl peroxide or methyl ethyl ketone peroxide, or a combination of at least two thereof; The first solution and the second solution are mixed, and a terminator is added to obtain a passivation solution; The terminator includes any one or a combination of at least two of sodium dimethyldithiocarbamate, sodium polysulfide or sodium nitrite; Add the silane coupling agent while adding the terminator; The carbon steel is immersed in the passivation solution and dried to obtain an interpenetrating organic network-silicon network composite passivation film.

2. The method according to claim 1, characterized in that The silicon source includes sodium silicate and / or ethyl orthosilicate.

3. The method according to claim 1, characterized in that The first solvent comprises an aqueous solution of alcohol, and the mass ratio of the alcohol to water is 3-7:7-3.

4. The method according to claim 3, characterized in that The alcohol includes any one of methanol, ethanol or isopropanol, or a combination of at least two of them.

5. The method according to claim 1, characterized in that The mass ratio of the silicon source to the first solvent is 1:4-8.

6. The method according to claim 1, characterized in that The silicon source and the first solvent are mixed under stirring.

7. The method according to claim 6, characterized in that The stirring speed is 300-800 rpm.

8. The method according to claim 6, characterized in that The stirring time is 1 to 3 hours.

9. The method according to claim 1, characterized in that: The second solvent includes water.

10. The method according to claim 1, characterized in that The mass ratio of the organic material to the silicon source is 1 to 2:

1.

11. The method according to claim 1, characterized in that: The mass ratio of the organic material to the second solvent is 1:3-5.

12. The method according to claim 1, characterized in that The mass ratio of the organic material to the initiator is 1:0.001-0.

01.

13. The method according to claim 1, characterized in that The initiator is added and stirred.

14. The method according to claim 13, characterized in that The stirring speed is 300-800 rpm.

15. The method according to claim 13, characterized in that The stirring temperature is 50-80°C.

16. The method according to claim 1, characterized in that The mass ratio of the organic material to the terminator is 1:0.001-0.

01.

17. The method according to claim 1, characterized in that The terminator is added and stirred.

18. The method according to claim 17, characterized in that The stirring speed is 300-800 rpm.

19. The method according to claim 17, characterized in that The stirring time is 1 to 3 hours.

20. The method according to claim 1, characterized in that The soaking time is 1 to 10 minutes.

21. The method according to claim 1, characterized in that The drying temperature is 100-150°C.