Thermally conductive silicone composition, method for producing the same, and semiconductor device
By using specific hydrolyzable groups and zinc oxide in the thermally conductive silicone composition, combining pH indicators and alkaline silane coupling agents, a composition with high thermal conductivity and good compressibility is achieved, and the prior art is solved The lack of thermally conductive silicone composition in the judgment of compression and thickening curing has improved the cooling efficiency and process management of electronic components.
Patent Information
- Application Number
- CN202180036731.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-22
- Filing Date
- 2021-05-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-05-11
AI Technical Summary
When the conventional thermally conductive silicone composition is compressed to a narrow thickness, the thermal conductivity decreases, the viscosity increases, making it difficult to effectively cool electronic components, and it is difficult to instantly judge the thickening or curing state, which affects the manufacturing and use of semiconductor devices.
The composition of organic polysiloxane, hydrolyzable silyl and zinc oxide containing hydroxyl groups or hydrolyzable groups is used, and the cross-linking reaction of atmospheric moisture is used by adding a pH indicator and an alkaline silane coupling agent. The color of the composition changes, thereby determining the thickening or curing state.
High thermal conductivity, good compression and high durability are achieved, effective cooling in semiconductor devices, and the thickening or curing state of the composition is instantly judged by color changes, thereby improving process management and assembly efficiency.
Smart Images

Figure BDA0003952863740000041 
Figure BDA0003952863740000042 
Figure BDA0003952863740000051
Abstract
Description
Technical Field
[0001] The present invention relates to a thermally conductive silicone composition, and more particularly to a thermally conductive silicone composition that can effectively cool an electronic component, a method for producing the composition, and a semiconductor device. Background Art
[0002] The heat generated during the use of electronic components and the resulting reduction in performance are widely known, and various heat dissipation technologies are used as means to solve them. Generally, heat is dissipated by arranging a cooling member (heat sink, etc.) near the heat generating portion, and effectively removing heat from the cooling member while keeping the two in close contact. At this time, if there is a gap between the heat generating member and the cooling member, the air with poor thermal conductivity is interposed between them, so the thermal resistance increases and the temperature of the heat generating member will not drop sufficiently. In order to prevent such a phenomenon, a heat dissipation material with good thermal conductivity and the ability to follow the surface of the component, such as a liquid heat dissipation material or a heat sink, is used. In particular, depending on the device, there is a situation where the gap is less than 10 μm and is very narrow, and a liquid heat dissipation material that can be compressed to less than 10 μm is used (Japanese Patent No. 2938428, Japanese Patent No. 2938429, Japanese Patent No. 3580366, Japanese Patent No. 3952184, Japanese Patent No. 4572243, Japanese Patent No. 4656340, Japanese Patent No. 4913874, Japanese Patent No. 4917380, Japanese Patent No. 4933094, Japanese Patent No. 2008-260798, Japanese Patent No. 2009-209165, Japanese Patent No. 2012-102283, Japanese Patent No. 2012-96361 (Patent Documents 1 to 13)).
[0003] In addition, there are many situations where the electrical insulation state must be ensured between the heating part and the cooling member, and insulation is sometimes required for the thermally conductive material. In this case, metal particles such as aluminum, copper, and silver cannot be used as thermally conductive fillers, and insulating thermally conductive fillers such as aluminum hydroxide and aluminum oxide (aluminum oxide) are mostly used. Aluminum hydroxide and aluminum oxide have low thermal conductivity, so if you want to use them to obtain a thermally conductive material with high thermal conductivity, you must fill them in large quantities. As a result, the viscosity of the thermally conductive material becomes very high and difficult to apply, it cannot be fully compressed, or the heat transfer distance becomes thicker (Japanese Patent Publication No. 2017-226724, Japanese Patent Publication No. 2017-210518 (Patent Documents 14, 15)).
[0004] Furthermore, it is known that the components repeatedly heat and shrink due to repeated heating and cooling of the heating part and the cooling member. This promotes the separation of the oil component of the thermally conductive silicone composition and the thermally conductive filler. In addition, phenomena such as the thermally conductive silicone composition being squeezed out from between the heating part and the cooling member may occur. As a result, the thermal resistance increases, and the heating part cannot be effectively cooled. In order to prevent such a phenomenon, a method of adding a thickener to increase the viscosity of the thermally conductive silicone composition has been proposed. However, there are problems such as the viscosity becoming very high and difficulty in coating (Japanese Patent Gazette No. 2004-91743 (Patent Document 16)).
[0005] Furthermore, when a silicone composition that thickens or cures using moisture in the atmosphere is filled or applied under actual semiconductor device manufacturing conditions, if the thickening or curing state of the composition after a certain period of time can be confirmed and judged without contacting the composition, it is expected that the process management will be improved and a storage place for components during assembly will not be required. Therefore, it is required to be able to judge the thickening and curing state of the composition applied to the semiconductor device in real time.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 2938428
[0009] Patent Document 2: Japanese Patent No. 2938429
[0010] Patent Document 3: Japanese Patent No. 3580366
[0011] Patent Document 4: Japanese Patent No. 3952184
[0012] Patent Document 5: Japanese Patent No. 4572243
[0013] Patent Document 6: Japanese Patent No. 4656340
[0014] Patent Document 7: Japanese Patent No. 4913874
[0015] Patent Document 8: Japanese Patent No. 4917380
[0016] Patent Document 9: Japanese Patent No. 4933094
[0017] Patent Document 10: Japanese Patent Application Publication No. 2008-260798
[0018] Patent Document 11: Japanese Patent Application Publication No. 2009-209165
[0019] Patent Document 12: Japanese Patent Application Publication No. 2012-102283
[0020] Patent Document 13: Japanese Patent Application Publication No. 2012-96361
[0021] Patent Document 14: Japanese Patent Application Publication No. 2017-226724
[0022] Patent Document 15: Japanese Patent Application Publication No. 2017-210518
[0023] Patent Document 16: Japanese Patent Application Publication No. 2004-91743 Summary of the invention
[0024] Problems to be solved by the invention
[0025] As described above, it is required to develop a thermally conductive silicone composition that has high thermal conductivity, compressibility to a thickness of less than 10 μm, and high durability (power cycle resistance, pump-out resistance). Furthermore, the goal is to develop a thermally conductive silicone composition that can immediately determine the thickening and curing conditions after application (filling, coating) to semiconductor devices, etc., especially whether the reaction related to thickening or curing is complete.
[0026] The present invention has been made in view of the above circumstances, and its object is to provide a thermally conductive silicone composition and a method for producing the same, as well as a semiconductor device. The thermally conductive silicone composition has higher thermal conductivity than conventional thermally conductive silicone compositions, can be compressed to a thickness of less than 10 μm, has high durability, and can visually recognize (judge) the thickening or curing state (i.e., the progress of the cross-linking reaction) after application (filling, coating) to a semiconductor device, etc.
[0027] Means for solving problems
[0028] As described above, it is required to develop a silicone composition that has high thermal conductivity and good compressibility when compressed to less than 10 μm, and further, it is required to develop a silicone composition that has a color (here, hue (color) and / or tone) that changes significantly from the initial color (unreacted color) when reacting with moisture (i.e., during a cross-linking reaction, especially when the cross-linking reaction is completed), so that the thickening or curing situation, especially the completion of the reaction related to the thickening or curing, can be visually recognized (judged).
[0029] The present inventors have conducted intensive studies on the above-mentioned problems and, as a result, have found that a silicone composition containing an organopolysiloxane having a hydroxyl group or a hydrolyzable group, a hydrolyzable organopolysiloxane having a specific hydrolyzable silyl group such as an alkoxysilyl group, a silicon compound having a hydrolyzable silyl group, and zinc oxide having an average particle size within a specific range has higher thermal conductivity than conventional silicone compositions and better compressibility when compressed to a thickness of 10 μm or less. In addition, by adding a pH indicator and a basic silane coupling agent, a silicone composition showing a clear color change accompanying a reaction related to thickening or curing can be prepared, thereby completing the present invention.
[0030] That is, the present invention provides the following thermally conductive silicone composition, a method for producing the same, and a semiconductor device. [1]
[0032] A thermally conductive silicone composition having a thermal conductivity of 0.5 W / mK or more at 25° C. using a hot plate method, comprising the following components (A) to (F):
[0033] (A) 100 parts by mass of an organopolysiloxane represented by the following general formula (1) or (2),
[0034] [Chemistry 1]
[0035]
[0036] (In the general formula (1), R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and n1 is an integer of 10 or more.)
[0037] [Chemistry 2]
[0038]
[0039] (In general formula (2), R 1 are independently an unsubstituted or substituted monovalent hydrocarbon group, Y is independently an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 Each of the following is independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms; m is independently an integer of 0 to 2 for each silicon atom to which it is bonded; and n2 is an integer greater than or equal to 10.
[0040] (B) an organopolysiloxane represented by the following general formula (3): 150 to 600 parts by mass,
[0041] [Chemistry 3]
[0042]
[0043] [In general formula (3), R 1 X is independently an unsubstituted or substituted monovalent hydrocarbon group. 1 For R 1 or-Y-SiR 2 g (OR 3 ) 3-g (wherein, Y is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 are independently alkyl, alkoxyalkyl, alkenyl or acyl having 1 to 4 carbon atoms, g is an integer of 0 to 2), 2 Independently by-Y-SiR 2 g (OR 3 ) 3-g (In the formula, Y, R 2 , R 3 , g and the above X 1 Y, R 2 , R 3 , g are the same) and contain at least one -Y-SiR 2 g (OR 3 ) 3-g a and b are integers satisfying the range of 1≤a≤1000 and 0≤b≤1000 respectively.]
[0044] (C) a crosslinking agent component of a hydrolyzable organosilane compound having one methyl group, vinyl group or phenyl group and at least three hydrolyzable groups in one molecule and / or a partially hydrolyzed condensate thereof: 0.1 to 100 parts by mass,
[0045] (D) zinc oxide particles having an average particle size of 0.1 μm or more and 2 μm or less, wherein the content of coarse powder having a particle size of 10 μm or more in laser diffraction type particle size distribution is 1% by volume or less of the total component (D): 1,500 to 6,500 parts by mass,
[0046] (E) Adhesion promoter: 0.01 to 30 parts by mass, and
[0047] (F) pH indicator: 0.01 to 20 parts by mass. [2]
[0049] The thermally conductive silicone composition according to [1] thickens or cures by a crosslinking reaction utilizing moisture in the atmosphere, and the color of the composition changes from a color in an unreacted state when the crosslinking reaction is completed. [3]
[0051] The thermally conductive silicone composition according to [1] or [2], wherein the content of the component (B) is 20 to 40% by volume based on the entire composition, and the composition can be compressed to a thickness of 10 μm or less. [4]
[0053] The thermally conductive silicone composition according to any one of [1] to [3], further comprising 0.01 to 20 parts by mass of (G) a reaction catalyst based on 100 parts by mass of the component (A). [5]
[0055] The thermally conductive silicone composition according to any one of [1] to [4], further comprising 1 to 1000 parts by mass of a (H) filler other than the (D) component, based on 100 parts by mass of the (A) component. [6]
[0057] The thermally conductive silicone composition according to any one of [1] to [5], wherein the thermal resistance at 25° C. measured by a laser flash method is 5 mm 2 ·K / W or less. [7]
[0059] The thermally conductive silicone composition according to any one of [1] to [6], wherein the viscosity of the thermally conductive silicone composition measured by a spiral viscometer at 25° C. and a shear rate of 6 S -1 The absolute viscosity is 3-600 Pa·S. [8]
[0061] The thermally conductive silicone composition according to any one of [1] to [7], which can suppress the deviation after a thermal cycle test. [9]
[0063] The thermally conductive silicone composition according to any one of [1] to [8], wherein the component (D) is surface-treated with the component (B).
[10]
[0065] The thermally conductive silicone composition according to any one of [1] to [9], wherein the component (E) is a basic silane coupling agent.
[11]
[0067] The thermally conductive silicone composition according to any one of [1] to
[10] , wherein the component (F) changes color in an alkaline region.
[12]
[0069] A method for producing a thermally conductive silicone composition according to any one of [1] to
[11] , comprising the step of mixing the components (A), (B), (C), (D), (E) and (F).
[13]
[0071] The method for producing a thermally conductive silicone composition according to
[12] , comprising: a step of mixing the component (B), or the components (A) and (B) together with the component (D) at a temperature of 100° C. or higher for 30 minutes or longer; and a step of mixing at least the components (C), (E) and (F) therein.
[14]
[0073] A semiconductor device characterized in that a gap having a thickness of 10 μm or less formed between a heating element and a cooling element is filled in a layered manner with the thermally conductive silicone composition according to any one of [1] to
[11] , wherein the composition layer is thermally conductively interposed between the heating element and the cooling element.
[15]
[0075] The semiconductor device according to
[14] is characterized in that the heat generating element is an insulated gate bipolar transistor.
[0076] Effects of the Invention
[0077] According to the present invention, a thermally conductive silicone composition having higher thermal conductivity than conventional thermally conductive silicone compositions, good compressibility when compressed to a thickness of 10 μm or less, and high durability (power cycle resistance, pump-out resistance) can be provided. Furthermore, the thermally conductive silicone composition changes color (from the color of the unreacted state) when the cross-linking reaction is completed in the composition, so after the composition is filled or applied to a semiconductor device, etc., it is thickened or cured at room temperature by using moisture in the atmosphere, and the color of the thermally conductive silicone composition changes from the color of the unreacted state immediately after application by visually confirming that the cross-linking reaction related to the thickening and curing of the thermally conductive silicone composition has been completed. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 This is a cross-sectional view showing an example of a semiconductor device in which the thermally conductive silicone composition of the present invention is interposed between an insulated gate bipolar transistor and a cooling fin. DETAILED DESCRIPTION
[0079] The present invention is a thermally conductive silicone composition comprising:
[0080] (A) 100 parts by mass of an organopolysiloxane represented by the following general formula (1) or (2),
[0081] [Chemistry 4]
[0082]
[0083] (In the general formula (1), R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and n1 is an integer of 10 or more.)
[0084] [Chemistry 5]
[0085]
[0086] (In general formula (2), R 1 are independently an unsubstituted or substituted monovalent hydrocarbon group, Y is independently an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 Each of the following is independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms; m is independently an integer of 0 to 2 for each silicon atom to which it is bonded; and n2 is an integer greater than or equal to 10.
[0087] (B) an organopolysiloxane represented by the following general formula (3): 150 to 600 parts by mass,
[0088] [Chemistry 6]
[0089]
[0090] [In general formula (3), R 1 X is independently an unsubstituted or substituted monovalent hydrocarbon group. 1 For R 1 or-Y-SiR 2 g (OR 3 ) 3-g (wherein, Y is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms, and g is an integer of 0 to 2. 2 Independently by-Y-SiR 2 g (OR 3 ) 3-g (In the formula, Y, R 2 , R 3 , g and the above X 1 Y, R 2 , R 3 , g are the same. ) represents a group containing at least one -Y-SiR 2 g (OR 3 ) 3-ga and b are integers satisfying the range of 1≤a≤1000 and 0≤b≤1000 respectively.]
[0091] (C) a crosslinking agent component of a hydrolyzable organosilane compound having one methyl group, vinyl group or phenyl group and at least three hydrolyzable groups in one molecule and / or a partially hydrolyzed condensate thereof: 0.1 to 100 parts by mass,
[0092] (D) zinc oxide particles having an average particle size of 0.1 μm or more and 2 μm or less, wherein the content of coarse powder having a particle size of 10 μm or more in laser diffraction type particle size distribution is 1% by volume or less of the total component (D): 1,500 to 6,500 parts by mass,
[0093] (E) Adhesion promoter: 0.01 to 30 parts by mass, and
[0094] (F) pH indicator: 0.01 to 20 parts by weight
[0095] , and further, may optionally contain
[0096] (G) a reaction catalyst,
[0097] (H) Fillers other than component (D)
[0098] The thermal conductivity of the thermally conductive silicone composition at 25°C using a hot plate method is 0.5 W / mK or more. More preferably, the thermally conductive silicone composition is compressible to a thickness of 10 μm or less, thickens or solidifies by a crosslinking reaction using atmospheric moisture, and when the crosslinking reaction is completed, the color of the composition changes from the color of the unreacted state. By thickening or solidifying using atmospheric moisture, the color of the unreacted state changes, so that it can be visually recognized (judged) that the reaction related to thickening or solidification has been completed.
[0099] Hereinafter, the present invention will be described in detail.
[0100] - (A) Component: Organopolysiloxane -
[0101] The component (A) is an organopolysiloxane represented by the following general formula (1). The organopolysiloxane has a structure in which both ends of the molecular chain are blocked by groups formed by bonding hydroxyl groups to silicon atoms, i.e., silanol groups or diorganohydroxysiloxy groups. The straight-chain organopolysiloxane of this structure functions as a main agent (base polymer) in the composition of the present invention.
[0102] [Chemistry 7]
[0103]
[0104] (In the general formula (1), R is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and a plurality of Rs may be the same as or different from each other. n1 is an integer greater than or equal to 10.)
[0105] In the above formula (1), the unsubstituted or substituted monovalent hydrocarbon group of R has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 8 carbon atoms.
[0106] As the unsubstituted monovalent hydrocarbon group of R, specifically, alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, cycloalkyl groups such as cyclopentyl and cyclohexyl, alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, pentenyl, hexenyl, aryl groups such as phenyl, tolyl, xylyl, α-, β-naphthyl, aralkyl groups such as benzyl, 2-phenylethyl, 3-phenylpropyl, etc. In addition, as the substituted monovalent hydrocarbon group of R, groups obtained by replacing part or all of the hydrogen atoms of the unsubstituted monovalent hydrocarbon group with halogen atoms such as fluorine (F), chlorine (Cl), bromine (Br), cyano, etc. can be mentioned. Examples of such groups include 3-chloropropyl, 3,3,3-trifluoropropyl, 2-cyanoethyl, etc. As R, among these unsubstituted or substituted monovalent hydrocarbon groups, methyl, ethyl, and phenyl are preferred, and methyl and phenyl are particularly preferred from the perspectives of availability, productivity, and cost.
[0107] In addition, the organopolysiloxane of the component (A) (formula (1) and formula (2) described later) is preferably an organopolysiloxane having a viscosity of 10 to 1,000,000 mPa·s at 25°C, more preferably an organopolysiloxane having a viscosity of 50 to 500,000 mPa·s, particularly preferably an organopolysiloxane having a viscosity of 100 to 200,000 mPa·s, and further preferably an organopolysiloxane having a viscosity of 500 to 100,000 mPa·s. If the viscosity of the above-mentioned organopolysiloxane at 25°C is 10 mPa·s or more, it is easy to obtain a coating film having excellent physical and mechanical strength, so it is preferred. If it is 1,000,000 mPa·s or less, the viscosity of the composition will not increase too much, and the operability during use is good, so it is preferred. Unless otherwise specified, the viscosity described in this specification is a value measured using a rotational viscometer. As a rotational viscometer, for example, a BL type, a BH type, a BS type, a cone-plate type, etc. rotational viscometer (the same below) can be cited.
[0108] The value of n1 in the above general formula (1) is the number of units or the degree of polymerization of the bifunctional diorganosiloxane present in the molecule. In the embodiment in which the organopolysiloxane of the component (A) can have a viscosity within the above preferred range, the number of units or the degree of polymerization of the bifunctional diorganosiloxane represented by n1 in the general formula (1) is an integer of 10 to 2000, preferably 50 to 1800, more preferably 100 to 1700, and even more preferably 200 to 1600. It should be noted that the degree of polymerization (or molecular weight) described in this specification is obtained as the number average degree of polymerization (or number average molecular weight) calculated as polystyrene in gel permeation chromatography (GPC) analysis using toluene or the like as an elution solvent (the same below).
[0109] Alternatively, component (A) is an organopolysiloxane represented by the following general formula (2). This organopolysiloxane is a linear organopolysiloxane having hydrolyzable silyl groups having 1 to 3 organooxy groups bonded to silicon atoms at both ends of the molecular chain, and functions as a main agent (base polymer) in the composition of the present invention.
[0110] [Chemistry 8]
[0111]
[0112] (In general formula (2), R 1 are independently an unsubstituted or substituted monovalent hydrocarbon group, Y is independently an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 Each of the following is independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms; m is independently an integer of 0 to 2 for each silicon atom to which it is bonded; and n2 is an integer greater than or equal to 10.
[0113] In the above formula (2), R 1 It is independently an unsubstituted or substituted monovalent hydrocarbon group having preferably 1 to 10 carbon atoms, more preferably 1 to 6, and further preferably 1 to 3 carbon atoms. Examples thereof include straight-chain alkyl groups, branched-chain alkyl groups, cycloalkyl groups, alkenyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups. Examples of straight-chain alkyl groups include methyl groups, ethyl groups, propyl groups, hexyl groups, and octyl groups. Examples of branched-chain alkyl groups include isopropyl groups, isobutyl groups, tert-butyl groups, and 2-ethylhexyl groups. Examples of cycloalkyl groups include cyclopentyl groups and cyclohexyl groups. Examples of alkenyl groups include vinyl groups and allyl groups. Examples of aryl groups include phenyl groups and tolyl groups. Examples of aralkyl groups include 2-phenylethyl groups and 2-methyl-2-phenylethyl groups. Examples of halogenated alkyl groups include 3,3,3-trifluoropropyl groups, 2-(nonafluorobutyl)ethyl groups, and 2-(heptadecafluorooctyl)ethyl groups. As R 1 , preferably methyl, phenyl, vinyl, more preferably methyl.
[0114] Examples of the alkylene group having 1 to 4 carbon atoms for Y include straight-chain alkylene groups such as methylene, ethylene, propylene, and butylene, and isomers thereof such as isopropylene and isobutylene. Y is preferably an oxygen atom or an ethylene group.
[0115] R 2 They are independently unsubstituted or substituted monovalent hydrocarbon groups having preferably 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and still more preferably 1 to 3 carbon atoms, which do not contain an aliphatic unsaturated bond. Examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenyl; aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl; and groups in which a part or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms such as fluorine (F), chlorine (Cl), and bromine (Br), cyano, and the like, and a methyl group is particularly preferred.
[0116] The above R 3 Each of R is independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms. 3 For example, the alkyl group of R 1 The same alkyl groups as those exemplified above, having 1 to 4 carbon atoms, etc. Examples of the alkoxyalkyl group include methoxyethyl and methoxypropyl. Examples of the alkenyl group include the same alkyl groups as those for R 1 The exemplified alkenyl groups are the same alkenyl groups having 1 to 4 carbon atoms. 3 Examples of the acyl group include acetyl and propionyloxy. 3 An alkyl group is preferred, and a methyl group and an ethyl group are particularly preferred.
[0117] m is an integer of 0 to 2 independently for each silicon atom to which it is bonded, and is preferably 0. It should be noted that the molecule preferably has 1 to 6, particularly preferably 4 or 6, OR 3 base.
[0118] The value of n2 in the general formula (2) is the number of units or the degree of polymerization of the bifunctional diorganosiloxane present in the molecule. In the embodiment in which the organopolysiloxane of the component (A) can have a viscosity within the above-mentioned preferred range, the number of units or the degree of polymerization of the bifunctional diorganosiloxane represented by n2 in the general formula (2) is an integer of 10 to 2000, preferably 50 to 1800, more preferably 100 to 1700, and even more preferably 200 to 1600.
[0119] The organopolysiloxane of the component (A) may be used alone or in combination of two or more.
[0120] - (B) component: organopolysiloxane -
[0121] The component (B) is a hydrolyzable organopolysiloxane represented by the following general formula (3) and having a hydrolyzable silyl group such as an alkoxysilyl group at one end of the molecular chain and / or a side chain (non-end). The component (B) functions as a surface treatment agent (dispersant or wetting agent) for the zinc oxide particles (thermally conductive filler) of the component (D) described later. Therefore, as a result of the enhanced interaction between the component (B) and the zinc oxide particles of the component (D), even if the zinc oxide particles of the component (D) are filled in large quantities into the thermally conductive silicone composition, the thermally conductive silicone composition can maintain fluidity and suppress the reduction in heat dissipation performance caused by oil separation and pumping out over time.
[0122] [Chemistry 9]
[0123]
[0124] [In general formula (3), R 1 X is independently an unsubstituted or substituted monovalent hydrocarbon group. 1 For R 1 or-Y-SiR 2 g (OR 3 ) 3-g (wherein, Y is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 are independently alkyl, alkoxyalkyl, alkenyl or acyl having 1 to 4 carbon atoms, g is an integer of 0 to 2), 2 Independently by-Y-SiR 2 g (OR 3 ) 3-g (In the formula, Y, R 2 , R 3 , g and the above X 1 Y, R 2 , R 3 , g are the same) and contain at least one -Y-SiR 2 g (OR 3 ) 3-g a and b are integers satisfying the range of 1≤a≤1000 and 0≤b≤1000 respectively.]
[0125] In the above formula (3), R 1 With R in the above formula (2) 1Similarly, independently unsubstituted or substituted monovalent hydrocarbon groups preferably having 1 to 10 carbon atoms, more preferably 1 to 6, and further preferably 1 to 3 carbon atoms, examples of which include linear alkyl groups, branched alkyl groups, cycloalkyl groups, alkenyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups. Examples of linear alkyl groups include methyl groups, ethyl groups, propyl groups, hexyl groups, and octyl groups. Examples of branched alkyl groups include isopropyl groups, isobutyl groups, tert-butyl groups, and 2-ethylhexyl groups. Examples of cycloalkyl groups include cyclopentyl groups and cyclohexyl groups. Examples of alkenyl groups include vinyl groups and allyl groups. Examples of aryl groups include phenyl groups and tolyl groups. Examples of aralkyl groups include 2-phenylethyl groups and 2-methyl-2-phenylethyl groups. Examples of halogenated alkyl groups include 3,3,3-trifluoropropyl groups, 2-(nonafluorobutyl)ethyl groups, and 2-(heptadecafluorooctyl)ethyl groups. As R 1 , preferably methyl, phenyl and vinyl.
[0126] Examples of the alkylene group having 1 to 4 carbon atoms for Y include straight-chain alkylene groups such as methylene, ethylene, propylene, and butylene, and isomers thereof such as isopropylene and isobutylene. Y is preferably an oxygen atom or an ethylene group.
[0127] R 2 With R in the above formula (2) 2 Similarly, each is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and still more preferably 1 to 3 carbon atoms, which does not contain an aliphatic unsaturated bond. Examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenyl; aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl; and groups in which a part or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms such as fluorine (F), chlorine (Cl), and bromine (Br), cyano, and the like, and a methyl group is particularly preferred.
[0128] The above R 3 With R in the above formula (2) 3 Likewise, each of R is independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms. 3 For example, the alkyl group of R 1 The same alkyl groups as those exemplified above, having 1 to 4 carbon atoms, etc. Examples of the alkoxyalkyl group include methoxyethyl and methoxypropyl. Examples of the alkenyl group include the same alkyl groups as those for R 1 The exemplified alkenyl groups are the same alkenyl groups having 1 to 4 carbon atoms. 3 Examples of the acyl group include acetyl and propionyloxy. 3An alkyl group is preferred, and a methyl group and an ethyl group are particularly preferred.
[0129] a and b are as described above, a is preferably 10 to 1000, more preferably 10 to 300, b is preferably 0 to 100, more preferably 0 to 50, and particularly preferably 0. In addition, a+b is preferably 10 to 1000, more preferably 10 to 300, further preferably 12 to 100, and most preferably 14 to 50. When b=0, a is preferably 10 to 1000, more preferably 10 to 300, further preferably 12 to 100, and most preferably 14 to 50, and X 1 Y-SiR 2 g (OR 3 ) 3-g (In the formula, Y, R 2 , R 3 , g is the same as above). g is an integer of 0 to 2, preferably 0. It should be noted that it is preferred to have 1 to 6, particularly preferably 3, OR in the molecule. 3 It should be noted that the bonding order of each siloxane unit shown in the brackets is not particularly limited. In addition, the hydrolyzable organopolysiloxane of component (B) has a hydrolyzable silyl group such as an alkoxysilyl group at one end of the molecular chain and / or a side chain (non-end), and preferably has a hydrolyzable silyl group at least at one end of the molecular chain.
[0130] As suitable specific examples of the component (B), the following may be mentioned.
[0131] [Chemistry 10]
[0132]
[0133] The component (B) is the main component of the silicone matrix in the thermally conductive silicone composition of the present invention, and its content is 150 to 600 parts by mass, preferably 160 to 500 parts by mass, relative to 100 parts by mass of the component (A). In addition, the content of the component (B) is preferably 20 to 40% by volume, more preferably 25 to 35% by volume, relative to the entire thermally conductive silicone composition. By containing the component (B) within this range, good compressibility can be maintained while preventing deterioration of thermal resistance caused by oil separation and pumping out.
[0134] The content (volume %) of the component (B) relative to the total thermally conductive silicone composition is the volume ratio occupied in the composition. The volume of the component (B) can be obtained from the blending amount (mass) and density of the component (B), and the total volume of the thermally conductive silicone composition obtained from the blending amounts (mass) and densities of all the components is calculated. The content (volume %) of the component (B) relative to the total thermally conductive silicone composition can be obtained from {volume of the component (B)} / {total volume of the total thermally conductive silicone composition}×100(%).
[0135] Moreover, (B)component can be mix|blended individually by 1 type or in combination of 2 or more types.
[0136] - (C) component: cross-linking agent component -
[0137] The component (C) is a hydrolyzable organosilane compound other than the component (B) having one methyl, vinyl or phenyl group in one molecule and at least three hydrolyzable groups and / or a partially hydrolyzed condensate thereof (an organosiloxane oligomer having three or more residual hydrolyzable groups in a molecule produced by partially hydrolyzing and condensing the organosilane compound), wherein the hydrolyzable organosilane compound is represented by the formula: 4 -SiX3
[0138] (In the above formula, R 4 is any one group selected from methyl, vinyl and phenyl. X is a hydrolyzable group.
[0139] Indicated.
[0140] The component (C) is used as a crosslinking agent (chain extender). In addition, there is no amino group in the above-mentioned condensate as the component (C). It should be noted that an organosilane compound (SiR 4 2X2) and / or its partial hydrolysis condensate (an organosiloxane oligomer having two or more residual hydrolyzable groups in the molecule produced by partially hydrolyzing and condensing the organosilane compound).
[0141] Examples of the hydrolyzable group contained in the component (C) include alkoxy groups having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 4 carbon atoms, such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, and tert-butoxy; alkoxyalkoxy groups having 2 to 40 carbon atoms, preferably 2 to 10 carbon atoms, and more preferably 2 to 4 carbon atoms, such as methoxymethoxy and methoxyethoxy; alkenyloxy groups having 2 to 20 carbon atoms, preferably 2 to 10 carbon atoms, and more preferably 2 to 5 carbon atoms, such as vinyloxy, allyloxy, propenyloxy, and isopropenyloxy; ketoximo groups having 3 to 20 carbon atoms, preferably 3 to 10 carbon atoms, and more preferably 3 to 6 carbon atoms, such as dimethylketoxime, diethylketoxime, and methylethylketoxime; and acyloxy groups having 2 to 20 carbon atoms, preferably 2 to 10 carbon atoms, and more preferably 2 to 5 carbon atoms, such as acetoxy.
[0142] As the specific examples of (C) component, methyl trimethoxy silane, methyl triethoxy silane, vinyl trimethoxy silane, vinyl triethoxy silane, vinyl triisopropoxy silane, methyl tri(methoxyethoxy) silane, vinyl tri(methoxyethoxy) silane, methyl tripropylene silane, vinyl triisopropylene silane, phenyl triisopropylene silane, methyl triacetoxy silane, vinyl triacetoxy silane, methyl tri(methyl ethyl ketoxime) silane, vinyl tri(methyl ethyl ketoxime) silane etc. and the partial hydrolysis condensation products of these hydrolyzable organosilanes can be listed. However, (C) component is not limited to these specific examples. As (C) component, one corresponding compound can be used alone, or two or more can be used in combination.
[0143] The content of the component (C) is 0.1 to 100 parts by mass, preferably 0.1 to 25 parts by mass, and more preferably 0.5 to 18 parts by mass, relative to 100 parts by mass of the organopolysiloxane of the component (A). When the content of the component (C) is less than 0.1 parts by mass, insufficient crosslinking occurs, and it is difficult to obtain a desired viscous composition. If it exceeds 100 parts by mass, the following problem arises: the mechanical properties of the physical properties of the obtained composition are reduced, which becomes economically disadvantageous.
[0144] - (D) ingredient: zinc oxide particles -
[0145] The thermally conductive silicone composition of the present invention contains (D) zinc oxide particles as a thermally conductive filler. Zinc oxide has a thermal conductivity as high as that of metal oxides such as aluminum oxide and magnesium oxide. Therefore, as long as the necessary and sufficient amount can be filled, a thermally conductive silicone composition with relatively high thermal conductivity can be obtained. The average particle size of the zinc oxide particles of the (D) component is greater than 0.1 μm and less than 2 μm, preferably greater than 0.2 μm and less than 1.5 μm. When the average particle size of the zinc oxide particles of the (D) component exceeds 2 μm, the compressibility of the obtained thermally conductive silicone composition is significantly deteriorated. In addition, if the average particle size of the (D) zinc oxide particles is less than 0.1 μm, the viscosity of the thermally conductive silicone composition increases significantly.
[0146] The above average particle size is based on the volume average particle size (cumulative average diameter D 50 (Median diameter) can be measured, for example, by using Microtrac MT330OEX manufactured by Nikkiso Co., Ltd. (the same applies hereinafter).
[0147] The content (ratio of content) of coarse powder (coarse particles) having a particle size of 10 μm or more in the laser diffraction type particle size distribution of the component (D) is 1% by volume or less of the total component (D). If the content of the coarse powder exceeds 1% by volume, the thickness of the thermally conductive silicone composition cannot be reduced to 10 μm or less when compressed. In order to obtain such a coarse powder content, it is preferred to perform classification treatment in advance by conventional means, or the zinc oxide powder (component (D)) having such a coarse powder content can be obtained as a commercial product in the form of zinc oxide grade 1, grade 2, grade 3, etc.
[0148] The content of the coarse powder can be easily determined by measuring the particle size distribution of the entire component (D) using a laser diffraction scattering method, for example, Microtrac MT330OEX manufactured by Nikkiso Co., Ltd. (hereinafter the same).
[0149] In the thermally conductive silicone composition of the present invention, 1500 to 6500 parts by mass, preferably 2000 to 6000 parts by mass of zinc oxide particles of component (D) are mixed with respect to 100 parts by mass of component (A). In addition, the component (D) is preferably contained in an amount of 45 to 70% by volume, more preferably 55 to 65% by volume, relative to the entire thermally conductive silicone composition. If the content of zinc oxide particles (D) is less than 1500 parts by mass or less than 45% by volume, the thermal conductivity of the thermally conductive silicone composition is reduced, and if it exceeds 6500 parts by mass or 70% by volume, the thermally conductive silicone composition is uneven.
[0150] The content (volume %) of the zinc oxide particles (D) relative to the total thermally conductive silicone composition is the volume ratio occupied in the composition. The volume of the component (D) can be obtained from the blending amount (mass) and density of the component (D), and the total volume of the thermally conductive silicone composition obtained from the blending amounts (mass) and densities of all the components can be calculated. The content (volume %) of the component (D) relative to the total thermally conductive silicone composition can be obtained from {volume of the component (D)} / {total volume of the total thermally conductive silicone composition}×100(%).
[0151] In the thermally conductive silicone composition of the present invention, it is preferred that the component (D) is surface-treated with the component (B).
[0152] - (E) ingredient: adhesion promoter -
[0153] The adhesion promoter of the component (E) is used to impart the necessary adhesion to the thermally conductive silicone composition of the present invention. As the adhesion promoter of the component (E), a known silane coupling agent (excluding the component (C)) is suitable. Examples of the silane coupling agent include hydrolyzable silanes containing carbon functional groups (so-called carbon functional silanes), and the like, such as (meth) acrylic silane coupling agents, epoxy silane coupling agents, amino silane coupling agents (however, excluding hydrolyzable silane compounds containing guanidine groups), mercapto silane coupling agents, and isocyanate silane coupling agents.
[0154] Specifically, examples include γ-methacryloxypropyltrimethoxysilane; β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane; aminoalkyl-substituted alkoxysilanes such as 3-aminopropyltriethoxysilane and N-β(aminoethyl)γ-aminopropyltrimethoxysilane; γ-mercaptopropyltrimethoxysilane, isocyanate silane, and the like, as well as compounds obtained by partially hydrolyzing and condensing these.
[0155] Among the specific examples of these (E) components, basic silane coupling agents are preferred, and in particular, epoxy silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane are preferred; aminosilanes such as 3-aminopropyltriethoxysilane and N-β(aminoethyl)γ-aminopropyltrimethoxysilane are preferred; isocyanate silanes, and aminosilanes such as 3-aminopropyltriethoxysilane and N-β(aminoethyl)γ-aminopropyltrimethoxysilane are more preferred; isocyanate silanes, and aminosilanes such as 3-aminopropyltriethoxysilane and N-β(aminoethyl)γ-aminopropyltrimethoxysilane are further preferred, and aminoalkyltriethoxysilanes such as 3-aminopropyltriethoxysilane are particularly preferred.
[0156] The content of the component (E) is 0.01 to 30 parts by mass, particularly preferably 0.1 to 20 parts by mass, relative to 100 parts by mass of the component (A). If the content of the component (E) is less than 0.01 parts by mass and is too small relative to 100 parts by mass of the component (A), sufficient pressure-sensitive adhesive properties cannot be imparted to the composition of the present invention. If it exceeds 30 parts by mass, the following problem arises: the mechanical properties of the physical properties produced by the obtained composition are reduced, which becomes economically disadvantageous.
[0157] -(F) Component: pH indicator-
[0158] The component (F) used in the thermally conductive silicone composition of the present invention is a pH indicator that changes color according to changes in pH, preferably in an alkaline region. The purpose of the component (F) is to impart a color-changing function by using the pH change of the composition when the composition is adsorbed with moisture in the atmosphere and the reaction of thickening and curing proceeds, by using the adhesion promoter (silane coupling agent) of the component (E), especially a basic silane coupling agent such as the above-mentioned aminosilane coupling agent (the system contains the pH indicator and the silane coupling agent).
[0159] As the component (F), a commonly used pH indicator can be used. For example, as the component (F), phenolphthalein, thymolphthalein, alizarin yellow R, cresolphthalein, cresol red, phenol red, bromothymol blue, etc. can be exemplified, and these can be used alone or in combination of two or more.
[0160] The amount of component (F) is 0.01 to 20 parts by mass, preferably 0.1 to 9 parts by mass, and more preferably 1 to 6 parts by mass, relative to 100 parts by mass of component (A). If the amount of component (F) is less than the lower limit of 0.01 parts by mass, the color change may not be fully obtained. In addition, if the amount of component (F) exceeds the upper limit of 20 parts by mass, the pH indicator may precipitate on the surface of the thermally conductive silicone composition or the appearance of the composition may deteriorate.
[0161] - (G) component: reaction catalyst -
[0162] The reaction catalyst of the component (G) is an optional component that can be added as needed. As the reaction catalyst of the component (G), a non-metallic organic catalyst and / or a metallic catalyst can be used. The component (G) has the function of accelerating the curing (increasing the viscosity) of the thermally conductive silicone composition of the present invention.
[0163] Among the reaction catalysts of component (G), there are no particular restrictions on non-metallic organic catalysts, and known substances can be used as curing (viscosity increase) accelerators for the thermally conductive silicone composition. Examples thereof include: phosphazene compounds such as N, N, N', N', N", N"-hexamethyl-N"'-(trimethylsilylmethyl)-phosphorimidate triamide; amine compounds or salts thereof such as hexylamine and dodecylamine phosphate; quaternary ammonium salts such as benzyltriethylammonium acetate; dialkylhydroxylamines such as dimethylhydroxylamine and diethylhydroxylamine; silanes and siloxanes containing guanidine groups such as N, N, N', N'-tetramethylguanidinopropyltrimethoxysilane, N, N, N', N'-tetramethylguanidinopropylmethyldimethoxysilane, and N, N, N', N'-tetramethylguanidinopropyltris(trimethylsiloxy)silane. In addition, the non-metallic organic catalyst can be used alone or in combination of two or more.
[0164] Among the reaction catalysts of the component (G), the metal catalysts are not particularly limited, and known catalysts can be used as a curing (viscosity increase) accelerator of the thermally conductive silicone composition. Examples include alkyltin ester compounds such as dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dioctoate, dioctyltin dineodecanoate, and di-n-butyldimethoxytin; titanates or titanium chelates such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetra(2-ethylhexyl)titanium, dipropoxybis(acetylacetonate)titanium, and isopropoxyoctanediol titanium; zinc naphthenate, zinc stearate, and zinc 2-ethyloctoate; aluminum alkoxide compounds such as aluminum isopropoxide and aluminum sec-butoxide; aluminum chelates such as alkylacetic acid diisopropoxide aluminum and ethyl bisacetoacetate monoacetylacetonate aluminum; organic metal compounds such as bismuth (III) neodecanoate, bismuth (III) 2-ethylhexanoate, bismuth (III) citrate, bismuth octoate, 2-ethylhexanoic acid iron, cobalt 2-ethylhexanoate, manganese 2-ethylhexanoate, and cobalt naphthenate; and lower fatty acid salts of alkali metals such as potassium acetate, sodium acetate, and lithium oxalate. The metal catalyst is not limited to these. The metal-based catalyst may be used alone or in combination of two or more.
[0165] The content of component (G) can be a small amount of catalyst. In the case of a reaction catalyst containing component (G), its content is 0.01 to 20 parts by mass relative to 100 parts by mass of component (A), and in particular, it is preferably 0.05 to 10 parts by mass, and more preferably 0.05 to 5 parts by mass. If the content of component (G) is less than 0.01 parts by mass, good curing reaction (viscosity increase) properties cannot be obtained, so the undesirable situation of slowing down the reaction rate occurs. If it exceeds 20 parts by mass, the reaction rate of the composition is too fast, so it is possible that the operable time after the composition is applied is shortened.
[0166] -(H) ingredient: filler-
[0167] The filler of the (H) component is an optional component that can be mixed as needed. The (H) component is a filler (inorganic filler and / or organic resin filler) other than the zinc oxide particles of the above-mentioned (D) component, which is used to give sufficient mechanical strength to the composition. As the filler of the (H) component, a known filler can be used. For example, micro-powdered silica, pyrogenic silica, precipitated silica, silica obtained by hydrophobizing the surface of these silicas with an organosilicon compound; glass beads; hollow glass spheres; transparent resin beads; silica aerogel; metal oxides such as diatomaceous earth, iron oxide, titanium oxide, and smoky metal oxides; wet silica or products obtained by silane treatment of their surfaces; reinforcing agents such as quartz powder, talc, zeolite, and bentonite; metal carbonates such as asbestos, glass fiber, carbon fiber, calcium carbonate, magnesium carbonate, and zinc carbonate; synthetic resin powders such as glass wool, micro-powdered mica, fused silica powder, polystyrene, polyvinyl chloride, and polypropylene. Among the fillers exemplified above, inorganic fillers such as silica, calcium carbonate, and zeolite are preferred, and pyrogenic silica and calcium carbonate whose surfaces have been hydrophobized are particularly preferred. It should be noted that the filler of component (H) does not include zinc oxide having a given average particle size as defined in component (D) above.
[0168] When the component (H) is contained, the content thereof is 1 to 1000 parts by mass, preferably 3 to 500 parts by mass, and particularly preferably 5 to 300 parts by mass, relative to 100 parts by mass of the component (A). If the amount used is more than 1000 parts by mass, the viscosity of the composition increases and the workability deteriorates. If the content of the component (H) is less than 1 part by mass, the mechanical strength of the obtained composition cannot be fully improved. The average particle size of the filler of the component (H) is preferably 0.005 μm (5 nm) or more and 2 μm or less, and more preferably 0.01 μm or more and 1.5 μm or less. It should be noted that, as for the filler of the component (H), the content (content ratio) of the coarse powder (coarse particles) with a particle size of 10 μm or more in the laser diffraction type particle size distribution is preferably 1% by volume or less of the total component (H). If the content of the coarse powder in the component (H) exceeds 1% by volume, it is sometimes difficult to make the thickness of the thermally conductive silicone composition when compressed to be 10 μm or less.
[0169] -Other ingredients: Organopolysiloxane-
[0170] The thermally conductive silicone composition of the present invention may contain (I) a linear diorganopolysiloxane represented by the following general formula (4) (so-called non-functional silicone oil) as an optional component in addition to the above components (A) to (H).
[0171] [Chemistry 11]
[0172]
[0173] In the general formula (4), R 5 It is a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms and not containing an aliphatic unsaturated bond which may have a substituent, and p is an integer of 1 to 2000.
[0174] In the above formula (4), R 5 The unsubstituted or substituted monovalent hydrocarbon group not containing an aliphatic unsaturated bond has 1 to 20 carbon atoms, preferably 1 to 10, and more preferably 1 to 8 carbon atoms. 5 They may be the same or different from each other. 5 Examples of the unsubstituted monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, and eicosyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl, tolyl, xylyl, α- and β-naphthyl; and aralkyl groups such as benzyl, 2-phenylethyl, and 3-phenylpropyl. In addition, examples of the substituted monovalent hydrocarbon group include groups in which a part or all of the hydrogen atoms of the unsubstituted monovalent hydrocarbon group are replaced by halogen atoms such as fluorine (F), chlorine (Cl), and bromine (Br), cyano, and the like, such as 3-chloropropyl, 3,3,3-trifluoropropyl, and 2-cyanoethyl. Among them, methyl, ethyl, and phenyl are preferred, and methyl and phenyl are more preferred from the perspective of ease of acquisition, productivity, and cost. In particular, it is preferred that R in formula (4) 5 All of them are methyl groups, and dimethylpolysiloxane in which both ends of the molecular chain are blocked with trimethylsiloxy groups is preferred.
[0175] In formula (4), p is a numerical value indicating the degree of polymerization of component (I), and is an integer of 1 to 2000, and is particularly preferably 2 to 2000, and is more preferably 20 to 2000. When p is a numerical value within the above range, the viscosity of the diorganopolysiloxane of component (I) at 25° C. is 1.5 to 1,000,000 mPa·s, and is preferably 30 to 100,000 mPa·s.
[0176] When the component (I) is contained, its content is preferably 0.01 to 100 parts by mass, and more preferably 10 to 80 parts by mass, relative to 100 parts by mass of the component (A). If the amount of the component (I) is within the above range, it is preferred in that the mechanical properties and flame retardancy of the thermally conductive silicone composition of the present invention are not impaired. In addition, the elastic modulus and viscosity of the composition can be adjusted to be easy to handle in construction.
[0177] [Other ingredients]
[0178] The thermally conductive silicone composition of the present invention may contain a conventionally known antioxidant such as 2,6-di-tert-butyl-4-methylphenol as needed to prevent the thermally conductive silicone composition from deteriorating. Furthermore, a thixotropy imparting agent, a dye, a pigment, a flame retardant, an anti-precipitation agent, a thixotropy enhancing agent, etc. may be contained as needed.
[0179] [Physical properties of silicone composition]
[0180] The thermally conductive silicone composition of the present invention has higher thermal conductivity than conventional thermally conductive silicone compositions and has good compressibility when compressed to a thickness of 10 μm or less.
[0181] The thermal conductivity of the thermally conductive silicone composition of the present invention at 25° C. by a hot plate method is 0.5 W / mK or more, preferably 1.3 W / mK or more. The details of the method for measuring the thermal conductivity are, for example, the method of Examples described later.
[0182] The thermally conductive silicone composition of the present invention has good compressibility. The thickness of the thermally conductive silicone composition when pressurized at 4.1 MPa for 2 minutes is 10 μm or less, preferably in the range of 0.5 to 10 μm, and more preferably in the range of 0.5 to 5 μm. It should be noted that the details of the method for measuring the thickness when pressurized are, for example, the method of the embodiment described later.
[0183] The thermally conductive silicone composition of the present invention has both high thermal conductivity and good compressibility, and thus has low thermal resistance. The thermal resistance of the thermally conductive silicone composition is measured by laser flash method and is preferably 5 mm at 25°C. 2 ·K / W or less, more preferably 3mm 2 ·K / W. There is no particular lower limit, but as a physical issue, it can be set to 0.1 mm, for example. 2 ·K / W. When the thermal resistance is equal to or less than a given value, the thermal conductivity of the thermally conductive silicone composition is further improved. The details of the method for measuring the thermal resistance are, for example, the method of the examples described later.
[0184] The absolute viscosity of the thermally conductive silicone composition of the present invention measured at 25°C using a spiral viscometer is preferably 3 to 600 Pa·s, more preferably 10 to 600 Pa·s. If the absolute viscosity is 3 Pa·s or more, it is easy to maintain the shape and the operability becomes good. On the other hand, when the absolute viscosity is 600 Pa·s or less, it becomes easy to eject, so the operability becomes good. The absolute viscosity can be adjusted by blending the above-mentioned components. In the present invention, the absolute viscosity is measured at 25°C and a shear rate of 6S / cm2 using a spiral viscometer manufactured by, for example, MALCOM Co., Ltd.-1 The value below.
[0185] Here, in the thermally conductive silicone composition of the present invention, the mechanism of the color change accompanying thickening and curing is based on the color change caused by the pH indicator. Generally, the thermally conductive silicone composition of the present invention thickens and cures by the progress of the condensation reaction (crosslinking reaction) using the moisture (water) in the atmosphere. Therefore, when the composition is stored in an unreacted state, it is stored in a state isolated from the atmosphere (external air). However, during the condensation reaction, when the composition is exposed to the atmosphere containing moisture (water), by making the composition contain (coexist) a pH indicator and a silane coupling agent having specific acidity or alkalinity, when the composition absorbs moisture (water) in the atmosphere from the surface, the absorbed moisture (water) penetrates into the system of the composition (or cured product). When there is effective moisture in the system (in the composition or cured product), the color change occurs due to the change in pH caused by the coexistence of the moisture and the silane coupling agent. However, in a moisture-thickening and curing type composition before the condensation reaction starts and / or during the reaction (before the reaction is completed), the moisture in the atmosphere that penetrates into the composition system (in the matrix) from the surface of the composition until the reaction of the composition is completed is preferentially consumed by the curing reaction (condensation reaction) of the composition, so that effective moisture that contributes to the color development of the pH indicator does not exist in the system (in the matrix), and therefore no color change occurs until the reaction is completed, and color development occurs after the reaction is completed. That is, the thermally conductive silicone composition of the present invention changes from the color (hue (color) and / or color tone) of the composition itself without the influence of the color development of the pH indicator (usually, in the case of containing fillers such as inorganic fillers, it is white or the hue of the filler itself other than white caused by the presence of the filler) to the color developed by the pH indicator after the reaction is completed. Therefore, if the color change mechanism of the present invention is utilized, it is possible to visually recognize (distinguish) more clearly the unreacted and reacted (thickening, curing) states than in the prior art.
[0186] [Method for producing thermally conductive silicone composition]
[0187] The method for producing the thermally conductive silicone composition of the present invention will be described.
[0188] The method for producing the thermally conductive silicone composition of the present invention is a method for producing the thermally conductive silicone composition of the present invention, characterized by comprising a step of mixing the above-mentioned components (A), (B), (C), (D), (E) and (F).
[0189] In this case, it is preferred to include a step of mixing the component (B) or the components (A) and (B) together with the component (D) at a temperature of 100° C. or higher, preferably 150° C. or higher and 250° C. or lower, for 30 minutes or longer, preferably 40 minutes or longer and 6 hours or shorter.
[0190] Specifically, it is preferred to include a step of mixing the component (B) or the components (A) and (B) with the component (D) as described above, and a step of mixing at least the components (C), (E) and (F) and other optional components as needed.
[0191] That is, components (B) and (D) or components (A), (B) and (D) are mixed under reduced pressure in advance, and mixed under heating, specifically at 100 to 160° C., for about 30 minutes to about 3 hours. Then, components (C), (E) and (F) and other components as required are added to the mixture, and further mixed under normal pressure or reduced pressure, preferably under reduced pressure of 0.09 to 0.01 MPa. The composition of the present invention can be produced by mixing without heating, preferably at 60° C. or less, for usually 30 minutes to about 3 hours.
[0192] The mixing device is not particularly limited, and a mixer such as TRIMIX, TWIN MIX, planetary mixer (all registered trademarks of mixers manufactured by Inoue Seisakusho Co., Ltd.), ULTRA MIXER (registered trademark of mixers manufactured by Mizuho Industries Co., Ltd.), HIVIS DISPER MIX (registered trademark of mixers manufactured by Tokushiki Kagaku Kogyo Co., Ltd.) can be used. In addition, in order to crush the agglomeration of the (D) zinc oxide particles as the thermally conductive filler, a three-roll finishing treatment or the like can be performed.
[0193] According to this production method, a thermally conductive silicone composition having a higher thermal conductivity than conventional thermally conductive silicone compositions and having good compressibility that can be compressed to a thickness of 10 μm or less can be produced.
[0194] In addition, in the step of mixing the above-mentioned component (B), or components (A) and (B) with component (D), by mixing at a temperature of 100° C. or higher for 30 minutes or longer, component (D) is sufficiently surface-treated with component (B), thereby suppressing deterioration of thermal resistance over time.
[0195] As an example of another production method, the thermally conductive silicone composition of the present invention can be produced by mixing the above-mentioned components (A), (B), (C), (D), (E) and (F) under normal pressure or reduced pressure, preferably under reduced pressure of 0.09 to 0.01 MPa, and then further mixing the mixture for about 30 minutes to 3 hours without heating, preferably at 60° C. or less. When components other than (A), (B), (C), (D), (E) and (F) are added in the above-mentioned production method, they can be added at the beginning of mixing the components (A), (B), (C), (D), (E) and (F) under normal pressure or reduced pressure.
[0196] [Semiconductor devices]
[0197] The semiconductor device of the present invention is characterized in that a gap with a thickness of less than 10 μm formed between a heating element such as an insulated gate bipolar transistor (IGBT) and a cooling element is filled with the thermally conductive silicone composition of the present invention in a layered manner, and the composition layer is located between the heating element and the cooling element in terms of heat transfer. The thermally conductive silicone composition of the present invention is compressed to a thickness of less than 10 μm. As a result, it is expected that the cooling efficiency will be improved compared to conventional thermally conductive silicone compositions.
[0198] A cross-sectional view of a representative structure is shown in Figure 1 , but the present invention is not limited to this.
[0199] At once Figure 1 In the semiconductor device shown, a thermally conductive silicone composition layer 2 made of the thermally conductive silicone composition of the present invention is interposed between a heating element 1 and a cooling element 3. The cooling element 3 has an insulating layer 3a provided on a surface in contact with the thermally conductive silicone composition layer 2.
[0200] Here, the heat generating element 1 is preferably an insulated gate bipolar transistor (IGBT). If the heat generating element 1 is an IGBT, the semiconductor device can efficiently cool the IGBT.
[0201] The cooling body 3 is preferably a cooling fin made of a material having good thermal conductivity (a fin made of a flat plate and a protrusion for heat dissipation provided on a main surface of one side of the flat plate).
[0202] The insulating layer 3a is a thin film with a thickness of 10 to 1000 μm formed on the surface (the flat plate of the cooling fin) of the cooling body 3 (cooling fin) where the thermally conductive silicone composition layer 2 is provided and is made of an insulating material with good thermal conductivity such as silicon nitride, aluminum nitride, or diamond.
[0203] In addition, the thermally conductive silicone composition layer 2 is a layer formed by arranging the thermally conductive silicone composition of the present invention in a layered manner in the gap between the back side of the heating element 1 (IGBT) and the plane side of the cooling element 3 (cooling fin). The thickness of the thermally conductive silicone composition layer 2 is 10 μm or less, preferably in the range of 0.5 to 10 μm, and more preferably in the range of 0.5 to 5 μm.
[0204] By forming such a structure of the semiconductor device, the heat generated by the heating element 1 is transferred to the cooling element 3 via the thermally conductive silicone composition layer 2 and dissipated to the outside. Figure 1 In the case of , heat is dissipated to the cooling water 4 connected to the cooling body 3.
[0205] The method for manufacturing the semiconductor device of the present invention is not particularly limited. In order to make the thickness of the thermally conductive silicone composition less than 10 μm, it is preferably assembled at a pressure of 0.1 MPa or more, more preferably at a pressure of 4.0 MPa or more. By increasing the pressure when the thermally conductive silicone composition is pressed, the time required for compression can be reduced.
[0206] In addition, the thermally conductive silicone composition layer 2 disposed in a layered manner in the gap between the back side of the heating element 1 (IGBT) and the plane side of the cooling element 3 (cooling fin) changes color after a certain period of time after filling, so that it is possible to confirm and judge that the thickening or curing reaction has been completed without contacting the composition. At this time, if a part of the thermally conductive silicone composition layer 2 is disposed in a manner slightly exposed from the gap, or a plate coated with the thermally conductive silicone composition on another plate is placed in the same environment, it is easy to confirm the color change accompanying the completion of the reaction of the composition layer 2 after filling, so it is preferred.
[0207] Furthermore, the thermally conductive silicone composition of the present invention does not cause contact failure of electric or electronic components and is therefore useful as an insulating material or adhesive for electric or electronic components.
[0208] Example
[0209] The present invention is specifically described below with reference to the following examples and comparative examples, but the present invention is not limited to the following examples. It should be noted that the average particle size of the zinc oxide particles (D) and the content (volume %) of the coarse powder having a particle size of 10 μm or more in the component (D) were measured using Microtrac MT330OEX manufactured by Nikkiso Co., Ltd. using a laser diffraction type particle size distribution measurement method (laser diffraction scattering method).
[0210] The ingredients used are described below.
[0211] [(A) ingredient]
[0212] (A-1) dimethyl polysiloxane having a viscosity of 700 mPa·s at 25°C and having hydroxyl groups at both ends of the molecular chain (n1 in formula (1) = about 268)
[0213] (A-2) dimethyl polysiloxane having a viscosity of 20,000 mPa·s at 25°C and having hydroxyl groups at both ends of the molecular chain (n1 in formula (1) = about 615)
[0214] (A-3) dimethyl polysiloxane having a viscosity of 50,000 mPa·s at 25°C and having hydroxyl groups at both ends of the molecular chain (n1 in formula (1) = about 886)
[0215] (A-4) dimethyl polysiloxane having a viscosity of 100,000 mPa·s at 25°C and having hydroxyl groups at both ends of the molecular chain (n1 in formula (1) = about 1589)
[0216] (A-5) a dimethylpolysiloxane represented by the following formula (2-1) having a viscosity of 900 mPa·s at 25° C. and having trimethoxysilyl groups capping both ends of the molecular chain
[0217] (In formula (2), R 1 =R 3 = methyl, Y = O, m = 0, n2 = 285)
[0218] [Chemistry 12]
[0219]
[0220] [(B) ingredient]
[0221] (B-1) a dimethylpolysiloxane having one end blocked with a trimethoxysilyl group represented by the following formula
[0222] [Chemistry 13]
[0223]
[0224] (B-2) a dimethylpolysiloxane having one end blocked with a trimethoxysilyl group represented by the following formula
[0225] [Chemistry 14]
[0226]
[0227] (B-3) a dimethylpolysiloxane having one end blocked with a trimethoxysilyl group represented by the following formula
[0228] [Chemistry 15]
[0229]
[0230] (B') Dimethyl polysiloxane having no hydrolyzable group represented by the following formula (comparative product)
[0231] [Chemistry 16]
[0232]
[0233] [(C) ingredient]
[0234] (C-1) Phenyl triisopropenyloxysilane
[0235] (C-2) Vinyl triisopropylene silane
[0236] (C-3) Methyltrimethoxysilane
[0237] [(D) ingredient]
[0238] (D-1) Zinc oxide particles having an average particle size of 1.0 μm and a coarse powder of 10 μm or more and a content of 0.1% by volume or less
[0239] (D-2) Zinc oxide particles with an average particle size of 40.0 μm and a coarse powder of 10 μm or more accounting for 80% by volume or more (for comparison)
[0240] [(E) ingredient]
[0241] (E-1) 3-Aminopropyltriethoxysilane
[0242] [(F)INGREDIENT]
[0243] (F-1) Phenolphthalein
[0244] (F-2) Thymolphthalein
[0245] [(G) ingredient]
[0246] (G) N, N, N', N'-Tetramethylguanidinopropyltrimethoxysilane
[0247] [(H) ingredient]
[0248] (H) BET specific surface area is 130m 2 / g of dry-process silica (average particle size: about 15 nm, content of coarse powder with a particle size of 10 μm or more <0.1% by volume)
[0249] [Examples 1 to 22, Comparative Examples 1 to 5]
[0250] <Preparation of thermally conductive silicone composition>
[0251] The above components (A) to (H) were blended in the amounts shown in Tables 1 to 6 below by the method shown below to prepare thermally conductive silicone compositions.
[0252] Components (A), (B) and (D) were added to a 5-liter planetary mixer (manufactured by Inoue Seisakusho Co., Ltd.) and mixed at 170° C. for 1 hour. After cooling to room temperature, components (C), (E) and (F) were added and mixed to obtain a uniform mixture, thereby preparing a thermally conductive silicone composition.
[0253] Furthermore, the component (G) and the component (H) are added and mixed as necessary to prepare a thermally conductive silicone composition.
[0254] For each thermally conductive silicone composition obtained by the above method, absolute viscosity, thermal conductivity, compressibility, thermal resistance, thermal resistance after thermal cycling, and change in appearance color (hue) were measured by the following methods. The results are shown in Tables 1 to 6.
[0255] [Absolute viscosity]
[0256] The viscometer was measured at 25°C and a rotation speed (shear rate) of 6 s. -1 The absolute viscosity of the thermally conductive silicone composition is measured under the conditions of.
[0257] [Thermal conductivity]
[0258] The thermally conductive silicone composition was wrapped in a kitchen wrap, and the thermal conductivity of the purse-shaped test piece was measured by a hot plate method at 25°C using TPA-501 manufactured by Kyoto Electronics Industry Co., Ltd.
[0259] [Compressibility]
[0260] The manufactured thermally conductive silicone composition was sandwiched between two silicon wafers cut into a circle with a diameter of 1 mm, and the minimum thickness was measured after being pressed at 4.1 MPa for 2 minutes using Autograph AG-5KNZPLUS manufactured by Shimadzu Corporation. The minimum thickness was measured by using two metal plates (silicon wafers) and taking the total thickness of the two metal plates when compressed without anything between the metal plates as the initial value. After measuring the initial value, the thickness of the thermally conductive silicone composition sandwiched between the two metal plates (silicon wafers) was measured and compressed, and then the initial value (total thickness of the two metal plates) was subtracted from the thickness to measure the minimum thickness of the thermally conductive silicone composition.
[0261] [Thermal resistance]
[0262] The above-mentioned test piece (the test piece after pressurization in the above [Compressibility] (the test piece in which the thermally conductive silicone composition was sandwiched between two silicon wafers) was used to measure the thermal resistance at 25°C using a laser flash method-based thermal resistance measuring instrument (manufactured by NETZSCH, xenon flash analyzer; LFA447NanoFlash).
[0263] [Thermal resistance after thermal cycling]
[0264] The above-mentioned test piece (the test piece after pressurization in the above-mentioned [Compressibility] (the test piece in which the thermally conductive silicone composition was sandwiched between two silicon wafers) was subjected to a thermal shock test with -40°C × 30 minutes → 150°C × 30 minutes as one cycle for 1000 cycles using a thermal shock tester TSE-11A manufactured by ESPEC Co., Ltd., and then the thermal resistance was measured at 25°C using a thermal resistance measuring instrument based on the laser flash method (manufactured by NETZSCH, xenon flash analyzer; LFA447NanoFlash).
[0265] [Appearance color change]
[0266] Each thermally conductive silicone composition was poured into a mold and molded into a 2 mm thick sheet. The color of the sheet at the time of molding (initial) and after being placed in an atmosphere of 23±2°C and 50±5% RH for 5 days (after 5 days) were visually evaluated to confirm the color change. It should be noted that after being placed in an atmosphere of 23±2°C and 50±5% RH for 5 days, all sheets were found to be thickened, but even after being placed in an atmosphere of 23±2°C and 50±5% RH, no viscosity change or color change was found.
[0267] [Table 1]
[0268]
[0269] [Table 2]
[0270]
[0271] [Table 3]
[0272]
[0273] [Table 4]
[0274]
[0275] [Table 5]
[0276]
[0277] [Table 6]
[0278]
[0279] As can be seen from the results of Tables 1 to 6, in Examples 1 to 22 that meet the necessary conditions of the present invention, a thermally conductive silicone composition having high thermal conductivity and good compressibility to be compressed to less than 10 μm was obtained, and a change from the initial color could be confirmed when exposed to an atmosphere of 23±2°C and 50±5% RH for 5 days (when the cross-linking reaction is completed). On the other hand, in Comparative Example 1 that does not contain the component (F) of the present invention and does not use the component (B), a uniform thermally conductive silicone composition cannot be obtained. In addition, in Comparative Example 2 that does not contain the component (F), the component (B) is less than 20% by volume, and the thermally conductive filler (D) is more than 70% by volume, a uniform thermally conductive silicone composition cannot be obtained. Furthermore, in Comparative Example 3 that does not contain the component (F) and uses zinc oxide particles with an average particle size of 40 μm as a thermally conductive filler, the compressibility is reduced and the thermal resistance value is significantly deteriorated. In addition, in Comparative Example 4, which does not contain component (F), uses zinc oxide particles with an average particle size of 40 μm as a thermally conductive filler, and the content of the thermally conductive filler is less than 40% by volume, the compressibility is reduced and the thermal conductivity is greatly reduced. In Comparative Example 5, component (F) is not contained, and the contents of components (B) and (D) are small, so sufficient compressibility cannot be obtained, and the necessary conditions of minimum thickness and thermal conductivity cannot be satisfied at the same time. Regarding the color change of Comparative Examples 1 to 5, since pH indicator (F) was not added, it was confirmed that no color change occurred over time.
[0280] It should be noted that the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative, and technical solutions having substantially the same structure and exerting the same effects as the technical ideas described in the claims of the present invention are all within the technical scope of the present invention.
[0281] Description of Reference Numerals
[0282] 1 Heating element (IGBT)
[0283] 2 Thermally conductive silicone composition layer
[0284] 3 Cooling element (cooling fins)
[0285] 3a Insulation layer
[0286] 4 Cooling water
Claims
1. A thermally conductive silicone composition having a thermal conductivity of 1.3 W / mK or more at 25° C. using a hot plate method, comprising the following components (A) to (F): (A) 100 parts by mass of an organopolysiloxane represented by the following general formula (1) or (2), [Chemistry 1] In the general formula (1), R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, n1 is an integer of 10 or more, [Chemistry 2] In the general formula (2), R 1 are independently an unsubstituted or substituted monovalent hydrocarbon group, Y is independently an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms, m is independently an integer of 0 to 2 for each silicon atom to which it is bonded, and n2 is an integer greater than or equal to 10, (B) an organopolysiloxane represented by the following general formula (3): 150 to 600 parts by mass, [Chemistry 3] In the general formula (3), R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups, X 1 For R 1 or-Y-SiR 2 g (OR 3 ) 3-g The groups shown, in, Y is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, R 3 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms, g is an integer of 0 to 2, and X 2 Independently by-Y-SiR 2 g (OR 3 ) 3-g The group shown, wherein Y, R 2 , R 3 , g and the above X 1 Y, R 2 , R 3 , g are the same, and contain at least one -Y-SiR 2 g (OR 3 ) 3-g , a and b are integers satisfying the range of 1≤a≤1000, 0≤b≤1000, respectively. (C) a crosslinking agent component of a hydrolyzable organosilane compound having one methyl group, vinyl group or phenyl group and at least three hydrolyzable groups in one molecule and / or a partially hydrolyzed condensate thereof: 0.1 to 100 parts by mass, (D) zinc oxide particles having an average particle size of 0.1 μm or more and 2 μm or less, wherein the content of coarse powder having a particle size of 10 μm or more in laser diffraction type particle size distribution is 1% by volume or less of the total component (D): 1,500 to 6,500 parts by mass, (E) Adhesion promoter: 0.01 to 30 parts by mass, and (F) pH indicator: 0.01 to 20 parts by weight, The content of the component (B) is 20 to 40% by volume of the entire composition, and the content of the component (D) is 45 to 70% by volume of the entire composition.
2. The thermally conductive silicone composition according to claim 1, which thickens or cures by a cross-linking reaction utilizing moisture in the atmosphere, wherein the color of the composition changes from that of an unreacted state upon completion of the cross-linking reaction. 3 . The thermally conductive silicone composition according to claim 1 , which can be compressed to a thickness of 10 μm or less.
4. The thermally conductive silicone composition according to claim 1 or 2, in, (G) A reaction catalyst: 0.01 to 20 parts by mass is further contained based on 100 parts by mass of the (A) component.
5. The thermally conductive silicone composition according to claim 1 or 2, in, (H) filler other than (D) component: 1 to 1000 parts by mass based on 100 parts by mass of (A) component.
6. The thermally conductive silicone composition according to claim 1 or 2, in, Thermal resistance at 25°C measured by laser flash method is 5 mm 2 ·K / W or less.
7. The thermally conductive silicone composition according to claim 1 or 2, in, Measured by spiral viscometer at 25°C and shear rate 6S -1 The absolute viscosity is 3-600 Pa·S. The thermally conductive silicone composition according to claim 1 or 2, which is capable of suppressing deviation after a thermal cycle test.
9. The thermally conductive silicone composition according to claim 1 or 2, in, The component (D) is obtained by surface-treating the component (B).
10. The thermally conductive silicone composition according to claim 1 or 2, in, The component (E) is a basic silane coupling agent.
11. The thermally conductive silicone composition according to claim 1 or 2, in, The component (F) changes color in the alkaline region.
12. A method for producing a thermally conductive silicone composition, the method for producing a thermally conductive silicone composition according to any one of claims 1 to 11, comprising the step of mixing the components (A), (B), (C), (D), (E) and (F).
13. The method for producing a thermally conductive silicone composition according to claim 12, wherein include: A step of mixing the component (B), or the components (A) and (B) together with the component (D) at a temperature of 100° C. or higher for 30 minutes or longer; and a step of mixing at least the components (C), (E) and (F) therein.
14. Semiconductor devices, It is characterized in that The gap with a thickness of 10 μm or less formed between the heating element and the cooling element is filled in layers. The thermally conductive silicone composition according to any one of claims 1 to 11, wherein the composition layer is interposed between the heating element and the cooling element in terms of heat conduction.
15. The semiconductor device according to claim 14, It is characterized in that The heating element is an insulated gate bipolar transistor.