High temperature and salt resistant polyacrylamide and its preparation method and application

By introducing specific structural units and functional monomers into polyacrylamide, high-temperature and salt-resistant polyacrylamide is prepared, which solves the problem of the decrease in viscosity of polymer oil flooding under high temperature and high salt conditions, and achieves effective adjustment of reservoir depth Drive and adjust blockage.

CN115677920BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110859282.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-28
Publication Date
2024-11-19
Estimated Expiration
2041-07-28

AI Technical Summary

Technical Problem

The existing polymer oil flooding exhibits polymer chain curling and rapid degradation under high temperature and high salt conditions, resulting in a decrease in the viscosity of the aqueous solution and is unable to effectively enter the deep oil reservoir. The fluidity of other chemical agents in the high water-containing stage is poor and cannot achieve it. The purpose of deep driving.

Method used

A high-temperature and salt-resistant polyacrylamide is adopted, which contains specific structural units A, B and C, and is prepared by solution polymerization and hydrolysis reaction. Functional monomer Y and monomer X are added to improve their temperature and salt conditions. Viscosity and emulsification properties.

Benefits of technology

The high-temperature and salt-resistant polyacrylamide has a high viscosity under high temperature (100℃) and high mineralization degree (48000mg/L), which can effectively enter the reservoir depth, reduce the interface tension of the oil and water meter, and has good emulsification performance , achieve the purpose of deep driving and blockage adjustment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115677920B_ABST
    Figure CN115677920B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of oilfield chemicals, and discloses a high temperature and salt resistant polyacrylamide and a preparation method and application thereof. The high temperature and salt resistant polyacrylamide comprises a structural unit A, a structural unit B and a structural unit C; the structural unit A has a structure shown in formula (1), the structural unit B has a structure shown in formula (2), and the structural unit C has a structure shown in formula (3); based on the total weight of the high temperature and salt resistant polyacrylamide, the content of the structural unit A is 88-96% by weight, the content of the structural unit B is 2-10% by weight, and the content of the structural unit C is 1-5% by weight; #imgabs0# wherein R1, R2 and R3 are each independently H or -CH3, and X is F or Br. The high temperature and salt resistant polyacrylamide has a higher viscosity under high temperature and high salt conditions, can enter the deep part of the oil reservoir, and can reduce the interfacial tension of the oil-water surface, and has good emulsification performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oilfield chemicals, and in particular to a high temperature and salt resistant polyacrylamide and a preparation method and application thereof. Background Art

[0002] In tertiary oil recovery, the use of water-soluble polymer flooding has developed into an extremely important technology for improving oil recovery. Water-soluble polymers have good water solubility and viscosity-increasing properties. When added to water, they can significantly increase the viscosity of the aqueous solution, reduce the water / oil mobility ratio under the reservoir, and then increase the fluid swept volume and sweep efficiency, reduce the oil saturation in the swept area, and thus achieve the purpose of improving oil recovery. And with the continuous improvement of the degree of water injection development in my country's oil fields, the water content of the reservoir has also continued to increase, and the requirements of adjusting the water absorption profile in the deep part of the reservoir, forcing the liquid flow to turn, and improving the recovery rate of water injection development have been proposed.

[0003] The polymer used in polymer flooding is mainly partially hydrolyzed polyacrylamide, which has excellent viscosity-increasing properties under conventional reservoir conditions and shows good oil recovery effects. However, under high temperature and high salt conditions, the oil recovery effects are significantly reduced. This is because the polymer molecular chains will curl and rapidly degrade under high temperature and high salt conditions, resulting in a significant decrease in the viscosity of the aqueous solution. Other new chemical agents, such as strong gels, weak gels, and granular gels, generally have poor fluidity, especially in the face of serious flooding of oil wells in the extremely high water content stage and complex oil-water relationships. They cannot achieve the purpose of deep reservoir flooding and can only work in the vicinity of the implementation well, resulting in a short on-site implementation period and poor results. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a high temperature and salt-resistant polyacrylamide and a preparation method and application thereof. The high temperature and salt-resistant polyacrylamide has a higher viscosity under high temperature and high salt conditions, can enter deep into the oil reservoir, and can reduce the interfacial tension between the oil and water surfaces, and has good emulsification properties.

[0005] In order to achieve the above-mentioned object, the present invention provides a high temperature and salt resistant polyacrylamide on one hand, characterized in that the high temperature and salt resistant polyacrylamide comprises structural unit A, structural unit B and structural unit C;

[0006] The structural unit A has a structure shown in formula (1), the structural unit B has a structure shown in formula (2), and the structural unit C has a structure shown in formula (3); based on the total weight of the high temperature and salt resistant polyacrylamide, the content of the structural unit A is 88-96 weight%, the content of the structural unit B is 2-10 weight%, and the content of the structural unit C is 1-5 weight%;

[0007]

[0008] Wherein, R1, R2 and R3 are each independently H or -CH3, and X is F or Br.

[0009] The second aspect of the present invention provides a method for preparing high temperature and salt resistant polyacrylamide, characterized in that the method comprises:

[0010] (1) subjecting a monomer mixture to a polymerization reaction in water under solution polymerization conditions and in the presence of an initiator to obtain a copolymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure represented by formula (4), and the monomer Y has a structure represented by formula (5);

[0011] Based on the total amount of the monomer mixture, the amount of acrylamide is 88-96% by weight, the amount of the monomer X is 2-10% by weight, and the amount of the monomer Y is 1-5% by weight;

[0012]

[0013] (2) subjecting the copolymer colloid to a hydrolysis reaction to obtain a high temperature and salt resistant polyacrylamide;

[0014] wherein R2' and R3' are each independently H or -CH3, and X' is F or Br.

[0015] The third aspect of the present invention provides high temperature and salt resistant polyacrylamide prepared by the above method.

[0016] A fourth aspect of the present invention provides the use of the high temperature and salt resistant polyacrylamide as a displacement agent in an oil field.

[0017] Through the above technical scheme, the high temperature and salt resistant polyacrylamide and its preparation method and application provided by the present invention achieve the following beneficial effects:

[0018] The molecular chain of the high temperature and salt resistant polyacrylamide provided by the present invention contains the structural unit B from the monomer X and the structural unit C from the monomer Y, which greatly improves the heat resistance and salt resistance of the copolymer and the surface and interfacial activity, and can effectively enter the deep part of the high temperature and high salt oil reservoir to achieve the purpose of deep displacement. The high temperature and salt resistant polyacrylamide has a high viscosity under high temperature (100°C) and high mineralization (48000mg / L) conditions, can enter the deep part of the oil reservoir, and can reduce the oil-water surface interfacial tension, and has good emulsification performance.

[0019] Further, in the present invention, in the preparation process of high temperature and salt resistant polyacrylamide, functional monomer Y, functional monomer X and (methyl) acrylamide containing strong hydrophilic groups and lipophilic groups are polymerized. Specifically, functional monomer Y has a good emulsifying effect, plays a self-emulsifying role in the polymerization system, and under the action of promoter and urea, the polymerization activity of the monomer is significantly improved, and the structural units of the three copolymer monomers can be randomly distributed in the polymer chain, thereby making it have excellent viscosity and emulsification and oil washing ability. In addition, the introduction of functional monomer X can slow down the hydrolysis and degradation of the polymer chain in high temperature and high salt reservoirs, so that the copolymer molecular chains always maintain a larger hydraulic volume, so that the copolymer aqueous solution still maintains a high viscosity under high temperature and high salt conditions, thereby achieving the purpose of deep flooding and plugging under the reservoir. DETAILED DESCRIPTION

[0020] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0021] The first aspect of the present invention provides a high temperature and salt resistant polyacrylamide, characterized in that the high temperature and salt resistant polyacrylamide comprises a structural unit A, a structural unit B and a structural unit C;

[0022] The structural unit A has a structure shown in formula (1), the structural unit B has a structure shown in formula (2), and the structural unit C has a structure shown in formula (3); based on the total weight of the high temperature and salt resistant polyacrylamide, the content of the structural unit A is 88-96 weight%, the content of the structural unit B is 2-10 weight%, and the content of the structural unit C is 1-5 weight%;

[0023]

[0024] Wherein, R1, R2 and R3 are each independently H or -CH3, and X is F or Br.

[0025] The inventors of the present invention have found in their research that by simultaneously introducing structural unit B and structural unit C into the macromolecular structure of polyacrylamide and controlling the content of each structural unit within the above range, the obtained high-temperature and salt-resistant polyacrylamide has a higher viscosity under high temperature (100°C) and high mineralization (48000 mg / L) conditions, can reduce the interfacial tension between the oil and water surfaces, has good emulsification properties, can adapt to the environment of severe flooding of oil wells and complex oil-water relationships, and achieve the purpose of deep profile control.

[0026] Furthermore, based on the total weight of the high temperature and salt resistant polyacrylamide, the content of the structural unit A is 88-90 weight %, the content of the structural unit B is 5-8 weight %, and the content of the structural unit C is 3-5 weight %.

[0027] In the present invention, the total content of the structural unit A, the structural unit B and the structural unit C is 100 wt %.

[0028] In the present invention, the content of each structural unit in the copolymer can be tested by conventional methods in the prior art, such as infrared spectroscopy, nuclear magnetic resonance, and the amount of monomers added during the polymerization process.

[0029] In the present invention, the content of each structural unit in the polymer is determined by the monomer feed amount. Specifically, the feed ratio of each monomer actually participating in the polymerization is determined by testing the content of unreacted monomers, and then the content of each structural unit in the polymer is determined.

[0030] Furthermore, in the present invention, when the content of each unreacted monomer in the tested polymer is less than 0.02 wt%, it indicates that substantially all monomers participate in the polymerization reaction. Specifically, the content of the residual monomer is determined by liquid chromatography.

[0031] In a preferred embodiment of the present invention, R1, R2 and R3 are H, and X is F.

[0032] In the present invention, under high temperature (greater than 100°C) and high salt (mineralization is 48,000 mg / L) conditions, the apparent viscosity of the high temperature and salt resistant polyacrylamide aqueous solution is greater than 50 mPa·s, preferably greater than 60 mPa·s.

[0033] In the present invention, the apparent viscosity of the high temperature and salt resistant polyacrylamide aqueous solution is measured using a Brookfield viscometer. Specifically, the apparent viscosity of the high temperature and salt resistant polyacrylamide aqueous solution (mass concentration of 0.15 weight %) is measured at a specified test temperature (100°C) and mineralization (mineralization of 48,000 mg / L).

[0034] The second aspect of the present invention provides a method for preparing high temperature and salt resistant polyacrylamide, characterized in that the method comprises:

[0035] (1) subjecting a monomer mixture to a polymerization reaction in water under solution polymerization conditions and in the presence of an initiator to obtain a copolymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure represented by formula (4), and the monomer Y has a structure represented by formula (5);

[0036] Based on the total amount of the monomer mixture, the amount of acrylamide is 88-96% by weight, the amount of the monomer X is 2-10% by weight, and the amount of the monomer Y is 1-5% by weight;

[0037]

[0038] (2) subjecting the copolymer colloid to a hydrolysis reaction to obtain a high temperature and salt resistant polyacrylamide;

[0039] wherein R2' and R3' are each independently H or -CH3, and X' is F or Br.

[0040] In the present invention, (meth)acrylamide, the monomer X and the monomer Y are all commercially available.

[0041] In the present invention, the amount of the monomer mixture is 20-40 parts by weight relative to 100 parts by weight of water.

[0042] In the present invention, (methyl)acrylamide, a monomer X having a structure represented by formula (4) and a monomer Y having a structure represented by formula (5) are copolymerized to obtain a high temperature and salt resistant polyacrylamide. The copolymer can have a high viscosity under high temperature (100°C) and high mineralization (48000 mg / L) conditions, can penetrate deep into the oil reservoir, and can reduce the interfacial tension between the oil and water surfaces, and has good emulsification properties.

[0043] In one embodiment of the present invention, R2' and R3' are each independently H or -CH3, and X' is F.

[0044] Furthermore, based on the total weight of the monomer mixture, the amount of the (meth)acrylamide is 88-90% by weight, the amount of the monomer X is 5-8% by weight, and the amount of the monomer Y is 3-5% by weight.

[0045] According to the present invention, the conditions of the solution polymerization reaction include: the initiator is an oxidation-reduction system initiator; the reaction temperature is 10-20° C., the reaction time is 8-10 h, and the pH value is 6-8.

[0046] In the present invention, the conventional means in the prior art can be used, for example, by adding alkaline substances such as sodium hydroxide to adjust the pH value of the polymerization reaction system.

[0047] According to the present invention, the conditions for the solution polymerization reaction also include: being carried out under an inert atmosphere.

[0048] In the present invention, a conventional atmosphere capable of providing an inert environment in the art, such as nitrogen, may be used.

[0049] According to the present invention, the amount of the initiator is 0.015-0.15 parts by weight relative to 100 parts by weight of the monomer mixture.

[0050] According to the present invention, the oxidation-reduction system initiator is a persulfate oxidant and a sulfite reductant.

[0051] In the present invention, the oxidation-reduction system initiator can be a conventional oxidation-reduction system initiator in the art, preferably a persulfate oxidant and a sulfite reducer.

[0052] Specifically, the persulfate oxidant may be, for example, potassium persulfate, ammonium persulfate, etc. The sulfite may be, for example, potassium bisulfite, sodium bisulfite, etc. Preferably, relative to 100 parts by weight of the monomer mixture, the persulfate oxidant is 0.01-0.1 parts by weight; the sulfite reducing agent is 0.005-0.05 parts by weight.

[0053] According to the present invention, the conditions of the solution polymerization reaction also include: being carried out in the presence of a complexing agent, urea and a promoter.

[0054] In the present invention, the influence of impurities on polymerization activity can be significantly reduced through the complexing effect of the complexing agent, the introduction of urea significantly increases the water solubility of the copolymer, and the introduction of the accelerator can further improve the viscosity and emulsification properties of the prepared high temperature and salt resistant polyacrylamide.

[0055] According to the present invention, relative to 100 parts by weight of the monomer mixture, the complexing agent is 0.01-0.1 parts by weight, the urea is 0.5-5 parts by weight, and the accelerator is 0.05-0.5 parts by weight.

[0056] According to the present invention, the complexing agent is disodium ethylenediaminetetraacetate (EDTA-2Na), and the accelerator is 1,3-bis(4-methoxyphenyl)thiourea.

[0057] In the present invention, the hydrolysis reaction can be carried out under alkaline conditions, and the alkaline conditions can be achieved by adding sodium hydroxide granules and other substances. There is no particular limitation on the amount of alkaline substance added, and those skilled in the art can adjust it according to the needs of the reaction. Preferably, the conditions of the hydrolysis reaction include: a temperature of 80-90°C and a time of 2-3h.

[0058] Preferably, after the hydrolysis reaction, the reaction product is granulated, dried, crushed and sieved to obtain the high temperature and salt resistant polyacrylamide.

[0059] In a preferred embodiment of the present invention, the method for preparing high temperature and salt resistant polyacrylamide comprises:

[0060] 1) adding (meth)acrylamide into a reactor to prepare an aqueous solution, then adding monomer X, monomer Y, complex aqueous solution, urea and accelerator, adjusting the pH value, and stirring sufficiently to make it a stable solution;

[0061] 2) adding an oxidation-reduction system initiator, blowing in an inert gas to mix evenly, sealing and polymerizing to obtain a polymer colloid;

[0062] 3) Taking out the colloid, adding alkaline substances after granulation, mixing it evenly and then carrying out hydrolysis reaction;

[0063] 4) Granulating, drying, crushing and screening the hydrolysis reaction product to obtain high temperature and salt resistant polyacrylamide.

[0064] The third aspect of the present invention provides high temperature and salt resistant polyacrylamide prepared by the above method.

[0065] The high temperature and salt resistant polyacrylamide provided by the present invention has high viscosity under high temperature (100°C) and high mineralization (48000mg / L) conditions, can enter deep oil reservoirs, and can reduce oil-water surface interfacial tension, has good emulsification properties, and can be applied to profile control agents to achieve deep profile control.

[0066] A fourth aspect of the present invention provides the use of the high temperature and salt resistant polyacrylamide as a displacement agent in an oil field.

[0067] The present invention will be described in detail below by way of examples. In the following examples,

[0068] Unless otherwise specified, all raw materials were purchased from commercial sources. Among them, the monomer X represented by formula (4) (in X1, R2' is H; in Y1, R2' is CH3) was purchased from Sinopharm Chemical Reagent Co., Ltd., and the monomer Y represented by formula (5) (in Y1, R3' is H, X' is F; in Y2, R3' is H, X' is Br) was purchased from J.B. & K. S. Co., Ltd.

[0069] Example 1

[0070] 1) Add 264 g of acrylamide to a heat-insulating polymerization reaction bottle, add 900 g of deionized water to dissolve and prepare an aqueous solution, add 130 g of monomer X, 6 g of monomer Y1, 0.15 g of EDTA-2Na, 3 g of urea, and 0.75 g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, then add sodium hydroxide to adjust the pH to 6, and stir thoroughly to form a stable solution;

[0071] 2) At 15° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 30 g of a 1 wt % aqueous solution of potassium persulfate and 15 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 8 hours to obtain a polymer colloid;

[0072] 3) Take out the colloid, granulate it, add 33.8g of sodium hydroxide granules, mix well, and perform hydrolysis reaction at 85°C for 3 hours;

[0073] 4) The colloid particles are taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular high temperature and salt resistant polyacrylamide J1.

[0074] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide J1, the content of the structural unit A is 88 weight %, the content of the structural unit B is 10 weight % and the content of the structural unit C is 2 weight %.

[0075] Example 2

[0076] 1) Add 288g of acrylamide to a heat-insulating polymerization reaction bottle, add 900g of deionized water to dissolve and prepare an aqueous solution, add 16g of monomer X, 16g of monomer Y, 0.1g of EDTA-2Na, 5g of urea, and 0.9g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, then add sodium hydroxide to adjust the pH to 7.3, and stir thoroughly to form a stable solution;

[0077] 2) At 10° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 18 g of a 1 wt % aqueous solution of potassium persulfate and 9 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 9 hours to obtain a polymer colloid;

[0078] 3) Take out the colloid, granulate it, add 30.4g of sodium hydroxide granules, mix well, and then carry out hydrolysis reaction at 80°C for 3 hours;

[0079] 4) The colloid particles are taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular high temperature and salt resistant polyacrylamide J2.

[0080] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide J2, the content of the structural unit A is 96 weight %, the content of the structural unit B is 2 weight % and the content of the structural unit C is 2 weight %.

[0081] Example 3

[0082] 1) Add 267g acrylamide to a heat-insulating polymerization reaction bottle, add 900g deionized water to dissolve and prepare an aqueous solution, add 118g monomer X, 115g monomer Y, 0.03g EDTA-2Na, 15g urea, 1.5g 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 8.0, and stir thoroughly to form a stable solution;

[0083] 2) At 20° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 3 g of a 1 wt % aqueous solution of potassium persulfate and 1.5 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to pass through for five minutes and then stopped. After sealing, the solution was polymerized for 10 hours to obtain a polymer colloid;

[0084] 3) Take out the colloid, granulate it, add 30.2g of sodium hydroxide granules, mix well, and then carry out hydrolysis reaction at 90°C for 2.5 hours;

[0085] 4) The colloid particles are taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular high temperature and salt resistant polyacrylamide J3.

[0086] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide J4, the content of the structural unit A is 89 weight %, the content of the structural unit B is 6 weight % and the content of the structural unit C is 5 weight %.

[0087] Example 4

[0088] 1) Add 273 g of acrylamide to a heat-insulating polymerization reaction bottle, add 900 g of deionized water to dissolve and prepare an aqueous solution, add 124 g of monomer X, 13 g of monomer Y, 0.22 g of EDTA-2Na, 1.5 g of urea, 1.2 g of 1,3-bis(4-methoxyphenyl)thiourea in sequence, add sodium hydroxide to adjust the pH to 7, and stir thoroughly to form a stable solution;

[0089] 2) At 17° C., nitrogen was passed through the solution to drive out oxygen for 30 minutes, and then 20 g of a 1 wt % aqueous solution of potassium persulfate and 10 g of a 1 wt % aqueous solution of sodium bisulfite were added to initiate the reaction. The nitrogen was continued to be passed through for five minutes and then stopped. After sealing, the solution was polymerized for 9 hours to obtain a polymer colloid;

[0090] 3) Take out the colloid, granulate it, add 33.2g of sodium hydroxide granules, mix well, and perform hydrolysis reaction at 90°C for 2 hours;

[0091] 4) The colloid particles are taken out and granulated, dried at 60° C. to constant weight, crushed, and sieved to obtain white granular high temperature and salt resistant polyacrylamide J4.

[0092] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide J3, the content of the structural unit A is 91 weight %, the content of the structural unit B is 8 weight % and the content of the structural unit C is 1 weight %.

[0093] Example 5

[0094] The high temperature and salt resistant polyacrylamide was prepared according to the method of Example 1, except that methacrylamide was used instead of acrylamide to obtain the high temperature and salt resistant polyacrylamide J5.

[0095] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide J5, the content of the structural unit A is 88 weight %, the content of the structural unit B is 10 weight % and the content of the structural unit C is 2 weight %.

[0096] Example 6

[0097] The high temperature and salt resistant polyacrylamide was prepared according to the method of Example 1, except that monomer X2 was used instead of monomer X1 to obtain high temperature and salt resistant polyacrylamide J6.

[0098] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide J6, the content of the structural unit A is 88 weight %, the content of the structural unit B is 10 weight % and the content of the structural unit C is 2 weight %.

[0099] Example 7

[0100] The high temperature and salt resistant polyacrylamide was prepared according to the method of Example 1, except that monomer Y2 was used instead of monomer Y1 to obtain high temperature and salt resistant polyacrylamide J7.

[0101] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide J7, the content of the structural unit A is 88 weight %, the content of the structural unit B is 10 weight % and the content of the structural unit C is 2 weight %.

[0102] Comparative Example 1

[0103] The high temperature and salt resistant polyacrylamide was prepared according to the method of Example 1, except that the monomer X with the same mass was used instead of the monomer Y to obtain the high temperature and salt resistant polyacrylamide D1.

[0104] According to the feed amount, based on the total weight of the high temperature and salt resistant polyacrylamide D1, the content of the structural unit A is 88 weight %, the content of the structural unit B is 12 weight % and the content of the structural unit C is 0 weight %.

[0105] Comparative Example 2

[0106] The high temperature and salt resistant polyacrylamide was prepared according to the method of Example 1, except that the monomer Y with the same mass was used instead of the monomer X to obtain the high temperature and salt resistant polyacrylamide D2.

[0107] According to the calculation determined by the feeding amount, based on the total weight of the high temperature and salt resistant polyacrylamide D2, the content of the structural unit A is 88 weight %, the content of the structural unit B is 0 weight % and the content of the structural unit C is 12 weight %.

[0108] Comparative Example 3

[0109] The high temperature and salt resistant polyacrylamide was prepared according to the method of Example 1, except that the amount of acrylamide used was 225 g, the amount of monomer X1 used was 45 g, and the amount of monomer Y1 used was 30 g, so as to obtain the high temperature and salt resistant polyacrylamide D3.

[0110] According to the feed amount, based on the total weight of the high temperature and salt resistant polyacrylamide D3, the content of the structural unit A is 75 weight %, the content of the structural unit B is 15 weight % and the content of the structural unit C is 10 weight %.

[0111] Test Case

[0112] The high temperature and salt resistant polyacrylamide obtained in the examples and comparative examples were respectively prepared into 0.15 wt % aqueous solutions, and the apparent viscosity, surface tension and interfacial tension of each aqueous solution were measured. The test results are shown in Table 1.

[0113] Among them, the apparent viscosity of the high temperature and salt resistant polyacrylamide aqueous solution was measured by Brookfield viscometer, the test temperature was 100 °C, and the mineralization was 48000 mg / L;

[0114] The surface tension of the high temperature and salt resistant polyacrylamide aqueous solution in pure water was measured by DCAT-21 surface tension meter, and the test temperature was 25℃;

[0115] The interfacial tension of the high temperature and salt resistant polyacrylamide aqueous solution was measured by TX500C interfacial tension meter of American Kono Company. The test temperature was 100℃ and the experimental oil was Shengli Oilfield crude oil.

[0116] Table 1

[0117] Product Number Apparent viscosity (mPa·s) Surface tension (mN / m) Interfacial tension (mN / m) J1 80.6 27.2 <![CDATA[5.6×10 -2 ]]> J2 78.4 28.7 <![CDATA[7.6×10 -2 ]]> J3 84.2 26.9 <![CDATA[4.5×10 -2 ]]> J4 75.1 29.2 <![CDATA[8.5×10 -2 ]]> J5 70.9 31.4 <![CDATA[8.8×10 -2 ]]> J6 64.8 31.5 <![CDATA[9.1×10 -2 ]]> J7 63.1 32.8 <![CDATA[8.6×10 -2 ]]> D1 48.2 68.4 4.5 D2 35.4 30.9 <![CDATA[8.7×10 -2 ]]> D3 39.8 31.6 <![CDATA[9.0×10 -2 ]]>

[0118] It can be seen from the results in Table 1 that the high temperature and salt-resistant polyacrylamide provided by the present invention has a higher apparent viscosity under the conditions of a temperature of 100°C and a mineralization of 48000 mg / L, showing excellent high temperature and high salt resistance; at the same time, it has lower surface tension and interfacial tension, showing excellent surface activity.

[0119] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing high temperature and salt resistant polyacrylamide, It is characterized in that The method includes: (1) subjecting a monomer mixture to a solution polymerization reaction in water under solution polymerization reaction conditions and in the presence of an initiator to obtain a copolymer colloid; wherein the monomer mixture comprises (meth)acrylamide, a monomer X and a monomer Y, wherein the monomer X has a structure represented by formula (4) and the monomer Y has a structure represented by formula (5); Based on the total amount of the monomer mixture, the amount of acrylamide is 88-96% by weight, the amount of the monomer X is 2-10% by weight, and the amount of the monomer Y is 1-5% by weight; Formula (4), Formula (5), (2) subjecting the copolymer colloid to a hydrolysis reaction to obtain a high temperature and salt resistant polyacrylamide; Among them, R 2 ' and R 3 ' are each independently H or -CH 3 , X' is F or Br; The conditions of the hydrolysis reaction include: temperature of 80-90° C. and time of 2-3 h.

2. The method according to claim 1, in, The conditions of the solution polymerization reaction include: the initiator is an oxidation-reduction system initiator; the reaction temperature is 10-20° C., the reaction time is 8-10 hours, and the pH value is 6-8.

3. The method according to claim 1, in, The conditions of the solution polymerization reaction also include: being carried out under an inert atmosphere.

4. The method according to claim 1, in, The amount of the initiator used is 0.015-0.15 parts by weight relative to 100 parts by weight of the monomer mixture.

5. The method according to claim 2, in, The oxidation-reduction system initiator is a persulfate oxidant and a sulfite reducer.

6. The method according to claim 5, in, Relative to 100 parts by weight of the monomer mixture, the persulfate oxidizing agent is 0.01-0.1 parts by weight; and the sulfite reducing agent is 0.005-0.05 parts by weight.

7. The method according to any one of claims 1 to 6, in, The conditions of the solution polymerization reaction also include: being carried out in the presence of a complexing agent, urea and a promoter.

8. The method according to claim 7, in, Relative to 100 parts by weight of the monomer mixture, the complexing agent is 0.01-0.1 parts by weight, the urea is 0.5-5 parts by weight, and the accelerator is 0.05-0.5 parts by weight.

9. The method according to claim 7, in, The complexing agent is disodium ethylenediaminetetraacetate, and the accelerator is 1,3-bis(4-methoxyphenyl)thiourea.

10. High temperature and salt resistant polyacrylamide prepared by the method according to any one of claims 1 to 9.