A recyclable flame-retardant epoxy resin and preparation method thereof

By mixing and curing itaconic acid-containing hyperbranched epoxy resin and hexahydrohomotriazine-terminal thiol hyperbranched polyether with bisphenol A-type epoxy resin, a flame retardant epoxy resin that can be recycled is prepared, and the problem is solved. The recycling problem of waste phosphorus-containing flame-retardant epoxy resin has achieved efficient recycling and improved flame-retardant performance of epoxy resin.

CN115678206BActive Publication Date: 2024-11-29SOUTH CENTRAL UNIVERSITY FOR NATIONALITIES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211413258.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-11-29
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle waste phosphorus-containing flame-retardant epoxy resin, resulting in waste of resources and environmental pollution. Thermoset polymers introduced by dynamic covalent bonds are prone to creep, have poor dimensional stability, and are difficult to apply in structural materials.

Method used

Itaconic acid-containing hyperbranched epoxy resin and hexahydrohomotriazine-terminal thiol hyperbranched polyether and bisphenol A-type epoxy resin were used to prepare a recyclable flame retardant epoxy resin, and through specific Reaction steps and process conditions improve their toughness and flame retardant properties.

Benefits of technology

It realizes efficient recycling and recycling of epoxy resin, has good mechanical properties and flame retardancy, has simple process and low raw material cost, and is suitable for construction, transportation, aerospace and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FHA0000006891290000021
    Figure FHA0000006891290000021
  • Figure FHA0000006891290000022
    Figure FHA0000006891290000022
  • Figure FHA0000006891290000023
    Figure FHA0000006891290000023
Patent Text Reader

Abstract

The present invention relates to the technical field of high-performance polymer resins, and in particular, to a recyclable flame-retardant epoxy resin and a preparation method thereof. The method prepares a phosphorus-containing itaconic acid hyperbranched epoxy resin and a hexahydro-s-triazine-terminated thiol hyperbranched polyester respectively, and then mixes and cures the bisphenol A type epoxy resin, the phosphorus-containing itaconic acid hyperbranched epoxy resin and the hexahydro-s-triazine-terminated thiol hyperbranched polyester to obtain a recyclable flame-retardant epoxy resin. The recyclable flame-retardant epoxy resin has good toughness and flame-retardant function, can be effectively recycled and recycled, has the advantage of environmental protection, and can be applied to the fields of construction, transportation, aerospace, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-performance polymer resins, and in particular to a recyclable flame-retardant epoxy resin and a preparation method thereof. Background Art

[0002] Organophosphorus flame retardants have high flame retardant efficiency, low smoke, toxic and corrosive gas generation, and have gradually replaced organohalogen flame retardants in the fields of epoxy resins. In 2020, China's organophosphorus flame retardant production was 294,200 tons, and the total domestic demand was 154,500 tons. In 2020, the market size of organophosphorus flame retardants in China reached 2.565 billion yuan. However, a large number of waste phosphorus-containing flame-retardant epoxy resin products after service are not put into substantial recycling every year. They are piled up in the open air for a long time, which not only occupies land resources, but also causes environmental problems such as groundwater pollution. Therefore, the rational recycling of phosphorus-containing flame-retardant epoxy resin products is not only related to the sustainable development of phosphorus chemical industry and epoxy resin industry, but also the need for comprehensive treatment of three wastes and comprehensive utilization of resources. Therefore, the recycling of phosphorus-containing flame-retardant epoxy resins has received widespread attention. At present, there are two main ways to recycle waste phosphorus-containing flame-retardant epoxy resin materials: physical method and chemical method. However, the physical and mechanical method has a low recycling rate, the thermal decomposition method consumes a lot of energy and pollutes the environment, the oxidation decomposition method and the solvent decomposition method use a large amount of oxidizing media and organic solvents, which can easily cause secondary pollution, and the super / subcritical fluid method requires harsh conditions for the medium to reach supercritical conditions and high equipment requirements.

[0003] By introducing dynamic covalent bonds into the molecular structure of thermosetting polymers, thermosetting polymers can achieve properties such as plastic deformation, welding, repeated processing and self-healing above the covalent bond exchange temperature. Chinese invention patent 202210157798.5 discloses a material and preparation method for a vanillin-based intrinsic flame-retardant epoxy resin, which solves the problem that the raw materials of traditional bisphenol A epoxy resins are non-renewable and the molecular structure causes brittleness and flammability. Chinese invention patent 202110888286.1 uses carboxylic acid-epoxy cross-linking reaction to obtain a recyclable flame-retardant epoxy resin. However, the introduction of dynamic covalent bonds will cause thermosetting polymers to be prone to creep and have poor dimensional stability, making them difficult to be used in structural materials. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a recyclable flame-retardant epoxy resin and a preparation method thereof.

[0005] The technical solution of the present invention to solve the above technical problems is as follows:

[0006] The invention provides a method for preparing a recyclable flame-retardant epoxy resin. The method comprises the following steps: preparing a phosphorus-containing itaconic acid hyperbranched epoxy resin and a hexahydro-s-triazine-terminated thiol hyperbranched polyether respectively; and then mixing and curing the bisphenol A epoxy resin, the phosphorus-containing itaconic acid hyperbranched epoxy resin and the hexahydro-s-triazine-terminated thiol hyperbranched polyether to obtain the recyclable flame-retardant epoxy resin.

[0007] Furthermore, the preparation method of the phosphorus-containing itaconic acid hyperbranched epoxy resin comprises the following steps:

[0008] S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, itaconic acid and a first organic solvent are uniformly mixed, and reacted at 40-80° C. for 1-4 hours; after the reaction is completed, the organic solvent is removed to obtain an itaconic acid adduct;

[0009] S1-2, the itaconic acid adduct, epichlorohydrin, the second organic solvent and the catalyst are mixed evenly, and reacted at 80-120° C. for 1-4 hours; then, an aqueous sodium hydroxide solution is added, and the reaction is continued at 20-40° C. for 2-4 hours; after the reaction is completed, the mixture is filtered, washed with water, and separated, and the organic layer is distilled under reduced pressure to obtain a phosphorus-containing itaconic acid epoxy resin;

[0010] In the sodium hydroxide aqueous solution, the mass of sodium hydroxide accounts for 10%-40% of the total mass of the solution;

[0011] S1-3, uniformly mixing the phosphorus-containing itaconic acid epoxy resin, the trivalent hydroxy compound and the catalyst, and reacting at 60-120° C. for 1-8 hours to obtain the phosphorus-containing itaconic acid hyperbranched epoxy resin.

[0012] Further, in the step S1-1, the mass ratio of the 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to the itaconic acid is 216:130;

[0013] The mass ratio of the 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to the first organic solvent is 1:(1.0-3.0);

[0014] The first organic solvent is one of xylene, tetrahydrofuran and propylene glycol methyl ether.

[0015] Further, in the step S1-2, the mass ratio of the itaconic acid adduct, the epichlorohydrin, the sodium hydroxide in the sodium hydroxide aqueous solution, and the second organic solvent is 1.0:(2.7-5.3):(0.2-0.5):(1.5-3.0);

[0016] The second organic solvent is one of ethyl acetate, methyl acetate or n-butyl acetate.

[0017] Further, in the step S1-3, the mass ratio of the phosphorus-containing itaconic acid epoxy resin, the trivalent hydroxy compound and the catalyst is 1.0:(0.08-0.30):(0.0001-0.001);

[0018] The trivalent hydroxy compound is one of trimethylolpropane, tris(2-hydroxyethyl)isocyanurate or glycerol;

[0019] The catalyst is one of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, hexadecyltriethylammonium bromide, benzyltriethylammonium chloride and trioctylmethylammonium chloride.

[0020] Furthermore, the structure of the phosphorus-containing itaconic acid hyperbranched epoxy resin is as shown in general formula (1), general formula (2) or general formula (3):

[0021]

[0022]

[0023] Among them, R 1 Expressed as In R 1 In the structural formula, * indicates the 3 The location of the connection;

[0024] R 2 Expressed as In R 2 In the structural formula, when R 2 With two R 3 When connected, ** and *** represent an R 3 Connected position, when R 2 R 3 and When connected, ** indicates that it is connected to R 3 The connection position, *** represents The location of the connection;

[0025] R 3 Expressed as **** represents and R 1 or R 2 The location of the connection.

[0026] Furthermore, the preparation method of the hexahydro-s-triazine thiol-terminated hyperbranched polyether comprises the following steps:

[0027] S2-1, 2-aminobenzenethiol, 30 wt% formaldehyde aqueous solution and a third organic solvent are mixed at 40-80° C. and reacted for 1-5 hours; after the reaction is completed, the mixture is filtered and the precipitate is dried at 40° C. for 4-6 hours to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine;

[0028] S2-2, first dissolving 2,2,2-(1,3,5)-triphenylthiol-s-triazine in a fourth organic solvent, then slowly dropping an alcohol solution of a divinyl monomer into the above solution, and reacting at 0°C-10°C for 1-3h; after the reaction, removing the fourth organic solvent to obtain the hexahydro-s-triazine-terminated thiol hyperbranched polyether;

[0029] Wherein, in the alcohol solution of divinyl monomer, the mass of divinyl monomer accounts for 10%-30% of the total mass of the solution.

[0030] Further, in the step 2-1, the mass ratio of the 2-aminothiophenol, formaldehyde and the third organic solvent is 1.0:(0.8-1.0):(2.5-3.5);

[0031] The third organic solvent is one of methanol, ethanol or isopropanol.

[0032] Further, the divinyl monomer is one of 1,4-cyclohexanedimethanol divinyl ether, diethylene glycol divinyl ether or tri(ethylene glycol) divinyl ether; the fourth organic solvent is one of dichloromethane, tetrahydrofuran or 1,4-dioxane; the alcohol solution of the divinyl monomer is ethanol, methanol or isopropanol solution of the divinyl monomer;

[0033] The mass ratio of the 2,2,2-(1,3,5)-triphenylthiol-s-triazine, the divinyl monomer and the fourth organic solvent is 1:(0.2-1.2):(0.6-1.4).

[0034] Furthermore, the structure of the hexahydro-s-triazine thiol-terminated hyperbranched polyether is shown in general formula (4), general formula (5) or general formula (6):

[0035]

[0036]

[0037] Among them, R 4 Expressed as R 4 In the structural formula, ***** represents -S-CH 2 - the location of the connection;

[0038] R 5 Expressed as R 5 In the structural formula of , ****** represents the position of connection with -S- or -SH.

[0039] Furthermore, the curing temperature is 80-120° C., and the curing time is 1-4 hours; the mass ratio of the bisphenol A epoxy resin, the phosphorus-containing itaconic acid hyperbranched epoxy resin, and the hexahydrotriazine-terminated mercapto hyperbranched polyether is 10.0:1.0.

[0040] The present invention also provides a recyclable flame-retardant epoxy resin, which is prepared by the above-mentioned preparation method.

[0041] The beneficial effects of the present invention are:

[0042] (1) The preparation method of the recyclable flame-retardant epoxy resin of the present invention uses a phosphorus-containing itaconic acid hyperbranched epoxy resin and a terminal mercapto group hexahydro-s-triazine hyperbranched polyester as raw materials. The phosphorus-containing itaconic acid hyperbranched epoxy resin has the functions of strengthening, toughening and flame retardant for the epoxy resin, and the terminal mercapto group hexahydro-s-triazine hyperbranched polyester realizes the recycling of the flame-retardant epoxy resin;

[0043] (2) The preparation method of the recyclable flame-retardant epoxy resin of the present invention has a simple preparation process, low raw material cost, and is easy to realize large-scale industrial production;

[0044] (3) The recyclable flame-retardant epoxy resin of the present invention has good mechanical properties and flame retardancy, and can be recycled and reused, which has the advantage of being environmentally friendly;

[0045] (4) The recyclable flame-retardant epoxy resin of the present invention has mild specific conditions for recycling and recycling and low cost;

[0046] (5) The recyclable flame-retardant epoxy resin of the present invention can be applied to the fields of construction, transportation, aerospace, etc. DETAILED DESCRIPTION

[0047] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0048] The invention discloses a method for preparing a recyclable flame-retardant epoxy resin. The method comprises the following steps: preparing a phosphorus-containing itaconic acid hyperbranched epoxy resin and a hexahydro-s-triazine-terminated thiol hyperbranched polyether respectively; and then mixing and curing the bisphenol A epoxy resin, the phosphorus-containing itaconic acid hyperbranched epoxy resin and the hexahydro-s-triazine-terminated thiol hyperbranched polyether to obtain the recyclable flame-retardant epoxy resin.

[0049] According to the preparation method of the present invention, the phosphorus-itaconic acid-containing hyperbranched epoxy resin has the functions of strengthening, toughening and flame retardant for epoxy resin, and the terminal mercapto hexahydro-s-triazine hyperbranched polyester realizes the recycling of flame retardant epoxy resin. The recyclable flame retardant epoxy resin obtained by the preparation method has the advantages of high efficiency recycling while ensuring the excellent mechanical and thermal properties of thermosetting resin. At the same time, the method also has the advantages of simple process, low raw material cost and easy large-scale industrial production.

[0050] In the preparation method of the present invention, the preparation method of the phosphorus-containing itaconic acid hyperbranched epoxy resin comprises the following steps:

[0051] S1-1. Evenly mix 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), itaconic acid and the first organic solvent, and stir to react at 40-80° C. for 1-4 h. After the reaction, remove the organic solvent by distillation under reduced pressure to obtain itaconic acid adduct DOPO-IA.

[0052] Preferably, the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) to itaconic acid is 216:130.

[0053] Preferably, the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) to the first organic solvent is 1:(1.0-3.0).

[0054] Preferably, the first organic solvent is one of xylene, tetrahydrofuran and propylene glycol methyl ether.

[0055] S1-2, the itaconic acid adduct DOPO-IA, epichlorohydrin, the second organic solvent and the catalyst are mixed evenly, and stirred at 80-120°C for 1-4h; then, an aqueous sodium hydroxide solution is added, and the reaction is continued at 20-40°C for 2-4h; after the reaction is completed, the mixture is filtered, washed with water, and separated, and the organic layer is distilled under reduced pressure to obtain a phosphorus itaconic acid epoxy resin (DOPO-E IA); in the aqueous sodium hydroxide solution, the mass of sodium hydroxide accounts for 10%-40% of the total mass of the solution.

[0056] Preferably, the mass ratio of itaconic acid adduct, epichlorohydrin, sodium hydroxide in sodium hydroxide aqueous solution, and the second organic solvent is 1.0:(2.7-5.3):(0.2-0.5):(1.5-3.0).

[0057] Preferably, the second organic solvent is one of ethyl acetate, methyl acetate or n-butyl acetate.

[0058] S1-3, uniformly mix the phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), the trivalent hydroxy compound and the catalyst, and stir the mixture at 60-120° C. for 1-8 hours to obtain the phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP).

[0059] Preferably, the mass ratio of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), trivalent hydroxy compound and the catalyst is 1.0:(0.08-0.30):(0.0001-0.001).

[0060] Preferably, the trivalent hydroxy compound is one of trimethylolpropane, tris(2-hydroxyethyl)isocyanurate or glycerol.

[0061] Preferably, the catalyst is one of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, hexadecyltriethylammonium bromide, benzyltriethylammonium chloride, and trioctylmethylammonium chloride.

[0062] The structure of the phosphorus-containing itaconic acid hyperbranched epoxy resin obtained in the above preparation process is shown in general formula (1), general formula (2) or general formula (3):

[0063]

[0064] Among them, R 1 Expressed as In R 1 In the structural formula, * indicates the 3 The location of the connection;

[0065] R 2 Expressed as In R 2 In the structural formula, when R 2 With two R 3 When connected, ** and *** represent an R 3 Connected position, when R 2 R 3 and When connected, ** indicates that it is connected to R 3 The connection position, *** represents The location of the connection;

[0066] R 3 Expressed as **** represents and R 1 or R 2 The location of the connection.

[0067] In the preparation method of the present invention, the preparation method of the hexahydro-s-triazine thiol-terminated hyperbranched polyether comprises the following steps:

[0068] S2-1. Mix 2-aminothiophenol (ATP), 30 wt% formaldehyde aqueous solution and a third organic solvent at 40-80°C and stir to react for 1-5 hours. After the reaction is completed, filter and dry the precipitate at 40°C for 4-6 hours to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0069] Preferably, the mass ratio of 2-aminothiophenol, formaldehyde and the third organic solvent is 1.0:(0.8-1.0):(2.5-3.5).

[0070] Preferably, the third organic solvent is one of methanol, ethanol or isopropanol.

[0071] S2-2, first dissolve 2,2,2-(1,3,5)-triphenylthiol-s-triazine in a fourth organic solvent, then slowly drop the alcohol solution of divinyl monomer into the above solution, and react at 0°C-10°C for 1-3h; after the reaction, remove the fourth organic solvent under reduced pressure to obtain the hexahydro-s-triazine terminal mercapto hyperbranched polyether.

[0072] Wherein, in the alcohol solution of divinyl monomer, the mass of divinyl monomer accounts for 10%-30% of the total mass of the solution.

[0073] Preferably, the divinyl monomer is one of 1,4-cyclohexanedimethanol divinyl ether, diethylene glycol divinyl ether or tri(ethylene glycol) divinyl ether; the fourth organic solvent is one of dichloromethane, tetrahydrofuran or 1,4-dioxane; and the alcohol solution of the divinyl monomer is an ethanol, methanol or isopropanol solution of the divinyl monomer.

[0074] Preferably, the mass ratio of 2,2,2-(1,3,5)-triphenylthiol-s-triazine, the divinyl monomer and the fourth organic solvent is 1:(0.2-1.2):(0.6-1.4).

[0075] The structure of the hexahydro-s-triazine thiol-terminated hyperbranched polyether prepared according to the above steps is shown in general formula (4), general formula (5) or general formula (6):

[0076]

[0077] Among them, R 4 Expressed as

[0078] R 4 In the structural formula, ***** represents -S-CH 2 - the location of the connection;

[0079] R 5 Expressed as R5 In the structural formula of , ****** represents the position of connection with -S- or -SH.

[0080] Preferably, in the preparation method of the present invention, the curing temperature is 80-120° C., and the curing time is 1-4 h; the mass ratio of bisphenol A epoxy resin, phosphorus-containing itaconic acid hyperbranched epoxy resin and hexahydrotriazine-terminated mercapto hyperbranched polyether is 10.0:1.0.

[0081] The recyclable flame-retardant epoxy resin of the present invention is prepared by adopting the above-mentioned preparation method.

[0082] The recyclable flame-retardant epoxy resin has good toughness and flame retardancy, and can also be effectively recycled and reused.

[0083] Specifically, the method for recycling the recyclable flame-retardant epoxy resin of the present invention is:

[0084] The recyclable flame-retardant epoxy resin of the present invention is placed in a 0.1 mol / L-0.5 mol / L acid solution and degraded at room temperature for 8-16 hours. The degradation liquid is filtered after adjusting the pH to 7 with a 10wt%-20wt% sodium hydroxide aqueous solution. The filtrate is subjected to rotary evaporation to remove the organic solvent to obtain recovered 2-aminothiophenol (r-ATP). The precipitate is adjusted to pH 2 with a 0.1 mol / L-0.5 mol / L acidic aqueous solution and dried at 20°C-40°C for 1-4 hours to obtain a recovered itaconic acid adduct (r-DOPO-IA).

[0085] The acid is one of phosphoric acid, acetic acid, formic acid or oxalic acid. The solvent of the acid solution is one of tetrahydrofuran, 1,4-dioxane or dimethylformamide. The mass ratio of the recyclable flame-retardant epoxy resin, the acid solution and the sodium hydroxide is 1.0:(10.0-20.0):(0.1-1.0).

[0086] The above-recovered 2-aminobenzenethiol (r-ATP), 30wt% formaldehyde aqueous solution and organic solvent are mixed at 40-80°C and stirred for reaction for 1-5h, and filtered after the reaction is completed. The precipitate is dried at 40°C for 4-6h to obtain the recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM). First, r-HT-BM is dissolved in an organic solvent, and then 10wt%-30wt% of the alcohol solution of divinyl monomer is slowly added dropwise to the above solution, and the reaction is carried out at 0°C-10°C for 1-3h. After the reaction is completed, the organic solvent is removed under reduced pressure to obtain the recovered hexahydro-s-triazine-terminated thiol hyperbranched polyether (r-THBP).

[0087] The mass ratio of 2-aminothiophenol (r-ATP), formaldehyde and organic solvent is 1.0: (0.8-1.0): (2.3-3.5). The divinyl monomer is one of 1,4-cyclohexanedimethanol divinyl ether, diethylene glycol divinyl ether or tri(ethylene glycol) divinyl ether. The mass ratio of r-HT-BM, divinyl monomer and organic solvent is 1: (0.2-1.2): (0.6-1.4). The organic solvent is one of methanol, ethanol, isopropanol, dichloromethane, tetrahydrofuran or 1,4-dioxane.

[0088] The above-mentioned recovered itaconic acid adduct r-DOPO-IA, epichlorohydrin, organic solvent and catalyst are mixed evenly and stirred at 80-120° C. for 1-4 hours, and then 10wt%-40wt% sodium hydroxide aqueous solution is added to continue the reaction at 20-40° C. for 2-4 hours. After the reaction is completed, it is filtered, washed with water, and separated. The organic layer is distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-EIA); the recovered phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), a trivalent hydroxy compound and a catalyst are mixed evenly and stirred at 60-120° C. for 1-8 hours to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP).

[0089] The mass ratio of r-DOPO-IA, epichlorohydrin, sodium hydroxide and organic solvent is 1.0:(2.7-5.3):(0.2-0.5):(1.5-3.0). The organic solvent is one of ethyl acetate, methyl acetate or n-butyl acetate, and the trivalent hydroxy compound is one of trimethylolpropane, tris(2-hydroxyethyl)isocyanurate or glycerol. The catalyst is one of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, hexadecyltriethylammonium bromide, benzyltriethylammonium chloride and trioctylmethylammonium chloride. The mass ratio of recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), trivalent hydroxy compound and catalyst is 1.0:(0.08-0.30):(0.0001-0.001).

[0090] Thus, the recyclable flame-retardant epoxy resin of the present invention can be completely degraded, and each product prepared and used can be restored to achieve complete recycling.

[0091] The method for recycling the recyclable flame-retardant epoxy resin of the present invention is:

[0092] The above-mentioned recycled bisphenol A epoxy resin, recycled phosphorus-containing itaconic acid hyperbranched epoxy resin and recycled hexahydrotriazine-terminated mercapto hyperbranched polyether are mixed and cured at 80-120° C. for 1-4 hours to obtain a recyclable flame-retardant epoxy resin, thereby realizing the recycling and reuse of the recyclable flame-retardant epoxy resin.

[0093] Among them, the mass ratio of bisphenol A epoxy resin, recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and recovered hexahydro-isotriazine terminal mercapto hyperbranched polyether is 10.0:1.0:(14.2-28.0).

[0094] The present invention is illustrated by means of specific embodiments below:

[0095] Example 1

[0096] Preparation of recyclable flame-retardant epoxy resin:

[0097] 216.0 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 130.0 g of itaconic acid and 216.0 g of tetrahydrofuran were mixed evenly, stirred at 60° C. for 3 h, and after the reaction was completed, tetrahydrofuran was removed by vacuum distillation to obtain itaconic acid adduct DOPO-IA.

[0098] 69.2 g of itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed evenly and stirred at 80°C for 4 hours. Then 60.0 g of 40 wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4 hours. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain phosphorus-containing itaconic acid epoxy resin (DOPO-EIA) with an epoxide value of 0.45 mol / 100 g.

[0099] 110.5 g of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), 16.8 g of trimethylolpropane and 0.8 g of tetrabutylammonium bromide were mixed evenly and stirred at 120°C for 6 h to obtain phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP). GPC test showed that its number average molecular weight was 10225 g / mol and the epoxide value was 0.12 mol / 100 g.

[0100] 62.5 g of 2-aminobenzenethiol (ATP), 50.0 g of 30 wt% formaldehyde aqueous solution and 405.0 g of ethanol were mixed at 80°C and stirred for reaction for 5 h. After the reaction was completed, the precipitate was filtered and dried at 40°C for 4-6 h to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0101] First, 102.8g HT-BM was dissolved in 63.8g dichloromethane, and then 245g 10wt% alcohol solution of 1,4-cyclohexanedimethanol divinyl ether was slowly added dropwise to the above solution. The reaction was carried out at 5°C for 2h. After the reaction was completed, the dichloromethane was removed under reduced pressure to obtain hexahydro-s-triazine terminal mercapto hyperbranched polyether. The molecular weight of the polyether was 5773g / mol as measured by GPC.

[0102] 100.0 g of bisphenol A epoxy resin, 10.0 g of phosphorus-containing itaconic acid hyperbranched epoxy resin and 251.1 g of hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0103] Recyclable flame retardant epoxy resin:

[0104] The recyclable flame-retardant epoxy resin was placed in 500.0 g of a 0.1 mol / L phosphoric acid / tetrahydrofuran solution and degraded at room temperature for 10 h. The degradation liquid was filtered after adjusting the pH to 7 with 60.0 g of a 10 wt% sodium hydroxide aqueous solution. The filtrate was evaporated to remove tetrahydrofuran to obtain recovered 2-aminothiophenol (r-ATP). The precipitate was adjusted to pH 2 with a 0.1 mol / L phosphoric acid aqueous solution and then dried at 20°C for 3 h to obtain a recovered itaconic acid adduct (r-DOPO-IA).

[0105] The above 62.5g of recovered 2-aminothiophenol (r-ATP), 50.0g of 30wt% formaldehyde aqueous solution and 405.0g of ethanol were mixed at 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was filtered and the precipitate was dried at 40°C for 4h to obtain recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM). First, 102.8g of r-HT-BM was dissolved in 63.8g of dichloromethane, and then 245g of 10wt% 1,4-cyclohexanedimethanol divinyl ether alcohol solution was slowly added dropwise to the above solution, and the mixture was reacted at 5°C for 2h. After the reaction was completed, the dichloromethane was removed under reduced pressure to obtain recovered hexahydro-s-triazine terminal thiol hyperbranched polyether, and its molecular weight was 5705g / mol as measured by GPC.

[0106] The above 69.2g of the recovered itaconic acid adduct r-DOPO-IA, 277.5g of epichlorohydrin, 105.6g of ethyl acetate and 0.6g of tetrabutylammonium bromide were mixed uniformly and stirred at 80°C for 4h, and then 60.0g of 40wt% sodium hydroxide aqueous solution was added to continue the reaction at 25°C for 4h. After the reaction was completed, it was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA) with an epoxy value of 0.45mol / 100g; 110.5g of the recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), 16.8g of trimethylolpropane and 0.8g of tetrabutylammonium bromide were mixed uniformly and stirred at 120°C for 6h to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP), and its number average molecular weight was 10117g / mol and its epoxy value was 0.12mol as measured by GPC. l / 100g.

[0107] Recycling of recyclable flame retardant epoxy resin:

[0108] Then, 100.0 g of bisphenol A epoxy resin, 10.0 g of recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and 248.2 g of recovered hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0109] Example 2

[0110] Preparation of recyclable flame-retardant epoxy resin:

[0111] 216.0 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 130.0 g of itaconic acid and 216.0 g of tetrahydrofuran were mixed evenly, stirred at 60° C. for 3 h, and after the reaction was completed, tetrahydrofuran was removed by vacuum distillation to obtain itaconic acid adduct DOPO-IA.

[0112] 69.2 g of itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed evenly and stirred at 80°C for 4 hours. Then 60.0 g of 40 wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4 hours. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain phosphorus-containing itaconic acid epoxy resin (DOPO-EIA) with an epoxide value of 0.45 mol / 100 g.

[0113] 110.5 g of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), 16.8 g of trimethylolpropane and 0.8 g of tetrabutylammonium bromide were mixed evenly and stirred at 120°C for 8 h to obtain phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP). GPC test showed that its number average molecular weight was 22195 g / mol and the epoxide value was 0.11 mol / 100 g.

[0114] 62.5 g of 2-aminobenzenethiol (ATP), 50.0 g of 30 wt% formaldehyde aqueous solution and 405.0 g of ethanol were mixed at 80°C and stirred for reaction for 5 h. After the reaction was completed, the precipitate was filtered and dried at 40°C for 4-6 h to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0115] First, 102.8 g of HT-BM was dissolved in 63.8 g of dichloromethane, and then 245 g of a 10 wt% alcohol solution of 1,4-cyclohexanedimethanol divinyl ether was slowly added dropwise to the above solution. The mixture was reacted at 5°C for 2 h. After the reaction, the dichloromethane was removed under reduced pressure to obtain a hexahydro-s-triazine-terminated mercapto hyperbranched polyether. The molecular weight of the polyether was 5773 g / mol as measured by GPC.

[0116] 100.0 g of bisphenol A epoxy resin, 10.0 g of phosphorus-containing itaconic acid hyperbranched epoxy resin and 250.6 g of hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0117] Recyclable flame retardant epoxy resin:

[0118] The recyclable flame-retardant epoxy resin was placed in a 500.0 g, 0.1 mol / L phosphoric acid / tetrahydrofuran solution and degraded at room temperature for 12 h. The degradation liquid was filtered after adjusting the pH to 7 with 30.0 g of a 20 wt% sodium hydroxide aqueous solution. The filtrate was evaporated to remove tetrahydrofuran to obtain recovered 2-aminothiophenol (r-ATP). The precipitate was adjusted to pH 2 with a 0.2 mol / L phosphoric acid aqueous solution and then dried at 20°C for 3 h to obtain a recovered itaconic acid adduct (r-DOPO-IA).

[0119] The above 62.5g of recovered 2-aminothiophenol (r-ATP), 50.0g of 30wt% formaldehyde aqueous solution and 405.0g of ethanol were mixed at 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was filtered and the precipitate was dried at 40°C for 4h to obtain recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM); 102.8g r-HT-BM was first dissolved in 63.8g of dichloromethane, and then 245g of a 10wt% alcohol solution of 1,4-cyclohexanedimethanol divinyl ether was slowly added dropwise to the above solution, and the mixture was reacted at 5°C for 2h. After the reaction was completed, the dichloromethane was removed under reduced pressure to obtain a recovered hexahydro-s-triazine-terminated thiol hyperbranched polyether, and its molecular weight was 5632g / mol as measured by GPC.

[0120] (9) The above 69.2 g of the recovered itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed uniformly and stirred at 80° C. for 4 h, and then 60.0 g of 40 wt % sodium hydroxide aqueous solution was added and the reaction was continued at 25° C. for 4 h. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA) with an epoxy value of 0.45 mol / 100 g; 110.5 g of the recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), 16.8 g of trimethylolpropane and 0.8 g of tetrabutylammonium bromide were mixed uniformly and stirred at 120° C. for 8 h to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP). The number average molecular weight of the recovered phosphorus-containing itaconic acid epoxy resin was 22046 g / mol and the epoxy value was 0.11 mol / 100 g by GPC test. l / 100g.

[0121] Recycling of recyclable flame retardant epoxy resin:

[0122] Then, 100.0 g of bisphenol A epoxy resin, 10.0 g of recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and 244.5 g of recovered hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0123] Example 3

[0124] Preparation of recyclable flame-retardant epoxy resin:

[0125] 216.0 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 130.0 g of itaconic acid and 212.0 g of xylene were mixed evenly, stirred and reacted at 60° C. for 3 h. After the reaction was completed, tetrahydrofuran was removed by vacuum distillation to obtain itaconic acid adduct DOPO-IA.

[0126] 69.2 g of itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed evenly and stirred at 80°C for 4 hours. Then 60.0 g of 40 wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4 hours. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain phosphorus-containing itaconic acid epoxy resin (DOPO-EIA) with an epoxide value of 0.45 mol / 100 g.

[0127] 110.5 g of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), 32.6 g of tris(2-hydroxyethyl)isocyanurate and 0.8 g of tetrabutylammonium bromide were mixed evenly and stirred at 120°C for 6 h to obtain phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP). GPC test showed that its number average molecular weight was 11092 g / mol and the epoxide value was 0.10 mol / 100 g.

[0128] 62.5 g of 2-aminobenzenethiol (ATP), 50.0 g of 30 wt% formaldehyde aqueous solution and 405.0 g of ethanol were mixed at 80°C and stirred for reaction for 5 h. After the reaction was completed, the precipitate was filtered and dried at 40°C for 4-6 h to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0129] First, 102.8g of HT-BM was dissolved in 63.8g of dichloromethane, and then 245g of a 10wt% alcohol solution of 1,4-cyclohexanedimethanol divinyl ether was slowly added dropwise to the above solution. The mixture was reacted at 5°C for 2h. After the reaction, the dichloromethane was removed under reduced pressure to obtain a hexahydro-s-triazine-terminated mercapto hyperbranched polyether. The molecular weight of the polyether was 5791g / mol as measured by GPC.

[0130] 100.0 g of bisphenol A epoxy resin, 10.0 g of phosphorus-containing itaconic acid hyperbranched epoxy resin and 250.9 g of hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0131] Recyclable flame retardant epoxy resin:

[0132] The recyclable flame-retardant epoxy resin was placed in 500.0 g of 0.1 mol / L phosphoric acid / tetrahydrofuran solution and degraded at room temperature for 10 h. The degradation liquid was filtered after adjusting the pH to 7 with 60.0 g of 10 wt% sodium hydroxide aqueous solution. The filtrate was evaporated to remove tetrahydrofuran to obtain recovered 2-aminothiophenol (r-ATP). The precipitate was adjusted to pH 2 with 0.1 mol / L phosphoric acid aqueous solution and then dried at 20°C for 3 h to obtain the recovered itaconic acid adduct (r-DOPO-IA).

[0133] The above 62.5g of recovered 2-aminothiophenol (r-ATP), 50.0g of 30wt% formaldehyde aqueous solution and 405.0g of ethanol were mixed at 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was filtered and the precipitate was dried at 40°C for 4h to obtain recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM); 102.8g r-HT-BM was first dissolved in 63.8g of dichloromethane, and then 245g of 10wt% alcohol solution of 1,4-cyclohexanedimethanol divinyl ether was slowly added dropwise to the above solution, and the mixture was reacted at 5°C for 2h. After the reaction was completed, the dichloromethane was removed under reduced pressure to obtain recovered hexahydro-s-triazine terminal thiol hyperbranched polyether, and its molecular weight was 5684g / mol as measured by GPC.

[0134] The above 69.2g of the recovered itaconic acid adduct r-DOPO-IA, 277.5g of epichlorohydrin, 105.6g of ethyl acetate and 0.6g of tetrabutylammonium bromide were mixed uniformly and stirred at 80°C for 4h, and then 60.0g of 40wt% sodium hydroxide aqueous solution was added to continue the reaction at 25°C for 4h. After the reaction was completed, it was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), and the epoxy value was 0.45mol / 100g; 110.5g of the recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), 32.6g of tris(2-hydroxyethyl)isocyanurate and 0.8g of tetrabutylammonium bromide were mixed uniformly and stirred at 120°C for 6h to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP), and its number average molecular weight was 10836g / mol by GPC test. l, epoxy value is 0.10mol / 100g.

[0135] Recycling of recyclable flame retardant epoxy resin:

[0136] Then, 100.0 g of bisphenol A epoxy resin, 10.0 g of recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and 246.3 g of recovered hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0137] Example 4

[0138] Preparation of recyclable flame-retardant epoxy resin:

[0139] 216.0 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 130.0 g of itaconic acid and 212.0 g of xylene were mixed evenly, stirred and reacted at 60° C. for 3 h. After the reaction was completed, tetrahydrofuran was removed by vacuum distillation to obtain itaconic acid adduct DOPO-IA.

[0140] 69.2 g of itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed evenly and stirred at 80°C for 4 hours. Then 60.0 g of 40 wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4 hours. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain phosphorus-containing itaconic acid epoxy resin (DOPO-EIA) with an epoxide value of 0.45 mol / 100 g.

[0141] 110.5 g of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), 16.8 g of trimethylolpropane and 0.8 g of tetrabutylammonium bromide were mixed evenly and stirred at 120° C. for 6 h to obtain phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP). GPC test showed that its number average molecular weight was 9846 g / mol and the epoxide value was 0.12 mol / 100 g.

[0142] 62.5 g of 2-aminobenzenethiol (ATP), 50.0 g of 30 wt% formaldehyde aqueous solution and 405.0 g of ethanol were mixed at 80°C and stirred for reaction for 5 h. After the reaction was completed, the precipitate was filtered and dried at 40°C for 4-6 h to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0143] First, 102.8 g of HT-BM was dissolved in 63.8 g of dichloromethane, and then 197.5 g of a 20 wt% alcohol solution of diethylene glycol divinyl ether was slowly added dropwise to the above solution. The mixture was reacted at 5°C for 2 h. After the reaction, the dichloromethane was removed under reduced pressure to obtain a hexahydro-s-triazine-terminated mercapto hyperbranched polyether. The molecular weight of the polyether was 5401 g / mol as measured by GPC.

[0144] 100.0 g of bisphenol A epoxy resin, 10.0 g of phosphorus-containing itaconic acid hyperbranched epoxy resin and 234.9 g of hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0145] Recyclable flame retardant epoxy resin:

[0146] The recyclable flame-retardant epoxy resin was placed in 900.0 g of 0.1 mol / L phosphoric acid / tetrahydrofuran solution and degraded at room temperature for 10 h. The degradation liquid was filtered after adjusting the pH to 7 with 108.0 g of 10 wt% sodium hydroxide aqueous solution. The filtrate was evaporated to remove tetrahydrofuran to obtain recovered 2-aminothiophenol (r-ATP). The precipitate was adjusted to pH 2 with 0.1 mol / L phosphoric acid aqueous solution and then dried at 20°C for 3 h to obtain the recovered itaconic acid adduct (r-DOPO-IA).

[0147] The above 62.5g of recovered 2-aminothiophenol (r-ATP), 50.0g of 30wt% formaldehyde aqueous solution and 405.0g of ethanol were mixed at 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was filtered and the precipitate was dried at 40°C for 4h to obtain recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM); 102.8g of r-HT-BM was first dissolved in 63.8g of dichloromethane, and then 197.5g of a 20wt% alcohol solution of diethylene glycol divinyl ether was slowly added dropwise to the above solution, and the mixture was reacted at 5°C for 2h. After the reaction was completed, the dichloromethane was removed under reduced pressure to obtain a recovered hexahydro-s-triazine-terminated thiol hyperbranched polyether, and its molecular weight was 5334g / mol as measured by GPC.

[0148] The above 69.2g of the recovered itaconic acid adduct DOPO-IA, 277.5g of epichlorohydrin, 105.6g of ethyl acetate and 0.6g of tetrabutylammonium bromide were mixed uniformly and stirred at 80°C for 4h, and then 60.0g of 40wt% sodium hydroxide aqueous solution was added to continue the reaction at 25°C for 4h. After the reaction was completed, it was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA) with an epoxy value of 0.45mol / 100g; 110.5g of the recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), 16.8g of trimethylolpropane and 0.8g of tetrabutylammonium bromide were mixed uniformly and stirred at 120°C for 6h to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP). The number average molecular weight of the recovered phosphorus-containing itaconic acid epoxy resin (r-IA-EHBP) was 9766g / mol and the epoxy value was 0.12mol by GPC test. l / 100g.

[0149] Recycling of recyclable flame retardant epoxy resin:

[0150] Then, 100.0 g of bisphenol A epoxy resin, 10.0 g of recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and 246.3 g of recovered hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0151] Example 5

[0152] Preparation of recyclable flame-retardant epoxy resin:

[0153] 216.0 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 130.0 g of itaconic acid and 212.0 g of xylene were mixed evenly, stirred and reacted at 60° C. for 3 h. After the reaction was completed, tetrahydrofuran was removed by vacuum distillation to obtain itaconic acid adduct DOPO-IA.

[0154] 69.2 g of itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed evenly and stirred at 80°C for 4 hours. Then 60.0 g of 40 wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4 hours. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain phosphorus-containing itaconic acid epoxy resin (DOPO-EIA) with an epoxide value of 0.45 mol / 100 g.

[0155] 110.5 g of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), 32.6 g of tris(2-hydroxyethyl)isocyanurate and 0.8 g of tetrabutylammonium bromide were mixed evenly and stirred at 120°C for 6 h to obtain phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP). GPC test showed that its number average molecular weight was 11092 g / mol and the epoxide value was 0.10 mol / 100 g.

[0156] 62.5 g of 2-aminobenzenethiol (ATP), 50.0 g of 30 wt% formaldehyde aqueous solution and 405.0 g of ethanol were mixed at 80°C and stirred for reaction for 5 h. After the reaction was completed, the precipitate was filtered and dried at 40°C for 4-6 h to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0157] First, 102.8g of HT-BM was dissolved in 110.0g of 1,4-dioxane, and then 84.3g of a 30wt% alcohol solution of tri(ethylene glycol) divinyl ether was slowly added dropwise to the above solution. The mixture was reacted at 5°C for 2h. After the reaction, the dichloromethane was removed under reduced pressure to obtain a hexahydro-s-triazine-terminated mercapto hyperbranched polyether. The molecular weight of the polyether was 5839g / mol as measured by GPC.

[0158] 100.0 g of bisphenol A epoxy resin, 10.0 g of phosphorus-containing itaconic acid hyperbranched epoxy resin and 253.0 g of hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0159] Recyclable flame retardant epoxy resin:

[0160] The above 50.0 g of recyclable flame-retardant epoxy resin was placed in 500.0 g of 0.5 mol / L phosphoric acid / tetrahydrofuran solution and degraded at room temperature for 8 h. The degradation liquid was filtered after adjusting the pH to 7 with 150.0 g of 20 wt% sodium hydroxide aqueous solution. The filtrate was evaporated to remove tetrahydrofuran to obtain recovered 2-aminothiophenol (r-ATP). The precipitate was adjusted to pH 2 with 0.1 mol / L phosphoric acid aqueous solution and then dried at 20°C for 3 h to obtain the recovered itaconic acid adduct (r-DOPO-IA).

[0161] The above 62.5g of recovered 2-aminothiophenol (r-ATP), 50.0gd of 30wt% formaldehyde aqueous solution and 405.0g of ethanol were mixed at 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was filtered and the precipitate was dried at 40°C for 4h to obtain recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM); 102.8g of r-HT-BM was first dissolved in 110.0g of 1,4-dioxane, and then 84.3g of 30wt% alcohol solution of tri(ethylene glycol) divinyl ether was slowly added dropwise to the above solution, and the mixture was reacted at 5°C for 2h. After the reaction was completed, 1,4-dioxane was removed under reduced pressure to obtain recovered hexahydro-s-triazine terminal thiol hyperbranched polyether, and its molecular weight was 5801g / mol as measured by GPC.

[0162] The above 69.2g of the recovered itaconic acid adduct DOPO-IA, 277.5g of epichlorohydrin, 105.6g of ethyl acetate and 0.6g of tetrabutylammonium bromide were mixed uniformly and stirred at 80°C for 4h, and then 60.0g of 40wt% sodium hydroxide aqueous solution was added to continue the reaction at 25°C for 4h. After the reaction was completed, it was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA) with an epoxide value of 0.45mol / 100g; 110.5g of the recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), 32.6g of tris(2-hydroxyethyl)isocyanurate and 0.8g of tetrabutylammonium bromide were mixed uniformly and stirred at 120°C for 6h to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP), and its number average molecular weight was 9896g / mol by GPC test. l, epoxy value is 0.10mol / 100g.

[0163] Recycling of recyclable flame retardant epoxy resin:

[0164] Then, 100.0 g of bisphenol A epoxy resin, 10.0 g of recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and 251.4 g of recovered hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0165] Example 6

[0166] Preparation of recyclable flame-retardant epoxy resin:

[0167] 216.0 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 130.0 g of itaconic acid and 212.0 g of xylene were mixed evenly, stirred and reacted at 60° C. for 3 h. After the reaction was completed, tetrahydrofuran was removed by vacuum distillation to obtain itaconic acid adduct DOPO-IA.

[0168] 69.2 g of itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed evenly and stirred at 80°C for 4 hours. Then 60.0 g of 40 wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4 hours. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain phosphorus-containing itaconic acid epoxy resin (DOPO-EIA) with an epoxide value of 0.45 mol / 100 g.

[0169] 110.5 g of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), 34.5 g of glycerol and 0.8 g of tetrabutylammonium bromide were mixed evenly and stirred at 120° C. for 4 h to obtain phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP). GPC test showed that its number average molecular weight was 4105 g / mol and the epoxide value was 0.14 mol / 100 g.

[0170] 62.5 g of 2-aminobenzenethiol (ATP), 50.0 g of 30 wt% formaldehyde aqueous solution and 405.0 g of ethanol were mixed at 80°C and stirred for reaction for 5 h. After the reaction was completed, the precipitate was filtered and dried at 40°C for 4-6 h to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0171] First, 102.8g HT-BM was dissolved in 63.8g dichloromethane, and then 197.5g of a 20wt% alcohol solution of diethylene glycol divinyl ether was slowly added dropwise to the above solution. The mixture was reacted at 5°C for 2h. After the reaction, the dichloromethane was removed under reduced pressure to obtain a hexahydro-s-triazine-terminated mercapto hyperbranched polyether. The molecular weight of the polyether was 5401g / mol as measured by GPC.

[0172] 100.0 g of bisphenol A epoxy resin, 10.0 g of phosphorus-containing itaconic acid hyperbranched epoxy resin and 235.8 g of hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0173] Recyclable flame retardant epoxy resin:

[0174] The recyclable flame-retardant epoxy resin was placed in 900.0 g of 0.1 mol / L phosphoric acid / tetrahydrofuran solution and degraded at room temperature for 10 h. The degradation liquid was filtered after adjusting the pH to 7 with 108.0 g of 10 wt% sodium hydroxide aqueous solution. The filtrate was evaporated to remove tetrahydrofuran to obtain recovered 2-aminothiophenol (r-ATP). The precipitate was adjusted to pH 2 with 0.1 mol / L phosphoric acid aqueous solution and then dried at 20°C for 3 h to obtain the recovered itaconic acid adduct (r-DOPO-IA).

[0175] The above 62.5g of recovered 2-aminothiophenol (r-ATP), 50.0g of 30wt% formaldehyde aqueous solution and 405.0g of ethanol were mixed at 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was filtered and the precipitate was dried at 40°C for 4h to obtain recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM); 102.8g r-HT-BM was first dissolved in 63.8g of dichloromethane, and then 197.5g of a 20wt% alcohol solution of diethylene glycol divinyl ether was slowly added dropwise to the above solution, and the mixture was reacted at 5°C for 2h. After the reaction was completed, the dichloromethane was removed under reduced pressure to obtain a recovered hexahydro-s-triazine terminal thiol hyperbranched polyether, and its molecular weight was 5386g / mol as measured by GPC.

[0176] The above 69.2g of the recovered itaconic acid adduct r-DOPO-IA, 277.5g of epichlorohydrin, 105.6g of ethyl acetate and 0.6g of tetrabutylammonium bromide were mixed uniformly and stirred at 80°C for 4h, and then 60.0g of 40wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4h. After the reaction was completed, it was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), and the epoxy value was 0.45mol / 100g; 110.5g of the recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), 34.5g of glycerol and 0.8g of tetrabutylammonium bromide were mixed uniformly and stirred at 120°C for 4h to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP), and its number average molecular weight was 4008g / mol and the epoxy value was 0.14mol by GPC test. l / 100g.

[0177] Recycling of recyclable flame retardant epoxy resin:

[0178] Then, 100.0 g of bisphenol A epoxy resin, 10.0 g of recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and 235.2 g of recovered hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0179] Example 7

[0180] Preparation of recyclable flame-retardant epoxy resin:

[0181] 216.0 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 130.0 g of itaconic acid and 212.0 g of xylene were mixed evenly, stirred and reacted at 60° C. for 3 h. After the reaction was completed, tetrahydrofuran was removed by vacuum distillation to obtain itaconic acid adduct DOPO-IA.

[0182] 69.2 g of itaconic acid adduct DOPO-IA, 277.5 g of epichlorohydrin, 105.6 g of ethyl acetate and 0.6 g of tetrabutylammonium bromide were mixed evenly and stirred at 80°C for 4 hours. Then 60.0 g of 40 wt% sodium hydroxide aqueous solution was added and the reaction was continued at 25°C for 4 hours. After the reaction was completed, the mixture was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain phosphorus-containing itaconic acid epoxy resin (DOPO-EIA) with an epoxide value of 0.45 mol / 100 g.

[0183] 110.5 g of phosphorus-containing itaconic acid epoxy resin (DOPO-E IA), 34.5 g of glycerol and 0.8 g of tetrabutylammonium bromide were mixed evenly and stirred at 120° C. for 4 h to obtain phosphorus-containing itaconic acid hyperbranched epoxy resin (IA-EHBP). GPC test showed that its number average molecular weight was 4105 g / mol and the epoxide value was 0.14 mol / 100 g.

[0184] 62.5 g of 2-aminobenzenethiol (ATP), 50.0 g of 30 wt% formaldehyde aqueous solution and 405.0 g of ethanol were mixed at 80°C and stirred for reaction for 5 h. After the reaction was completed, the precipitate was filtered and dried at 40°C for 4-6 h to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine (HT-BM).

[0185] First, 102.8 g of HT-BM was dissolved in 129.6 g of tetrahydrofuran, and then 63.0 g of a 20 wt% alcohol solution of tri(ethylene glycol) divinyl ether was slowly added dropwise to the above solution. The mixture was reacted at 5° C. for 2 h. After the reaction, the dichloromethane was removed under reduced pressure to obtain a hexahydro-s-triazine-terminated mercapto hyperbranched polyether. The molecular weight of the polyether was 5802 g / mol as measured by GPC.

[0186] 100.0 g of bisphenol A epoxy resin, 10.0 g of phosphorus-containing itaconic acid hyperbranched epoxy resin and 253.4 g of hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0187] Recyclable flame retardant epoxy resin:

[0188] The recyclable flame-retardant epoxy resin was placed in 900.0 g of 0.1 mol / L phosphoric acid / tetrahydrofuran solution and degraded at room temperature for 10 h. The degradation liquid was filtered after adjusting the pH to 7 with 108.0 g of 10 wt% sodium hydroxide aqueous solution. The filtrate was evaporated to remove tetrahydrofuran to obtain recovered 2-aminothiophenol (r-ATP). The precipitate was adjusted to pH 2 with 0.1 mol / L phosphoric acid aqueous solution and then dried at 20°C for 3 h to obtain the recovered itaconic acid adduct (r-DOPO-IA).

[0189] The above 62.5g of recovered 2-aminothiophenol (r-ATP), 50.0g of 30wt% formaldehyde aqueous solution and 405.0g of ethanol were mixed at 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was filtered and the precipitate was dried at 40°C for 4h to obtain recovered 2,2,2-(1,3,5)-triphenylthiol-s-triazine (r-HT-BM); 102.8g of r-HT-BM was first dissolved in 129.6g of tetrahydrofuran, and then 63.0g of 20wt% alcohol solution of tri(ethylene glycol) divinyl ether was slowly added dropwise to the above solution, and the mixture was reacted at 5°C for 2h. After the reaction was completed, the dichloromethane was removed under reduced pressure to obtain recovered hexahydro-s-triazine-terminated thiol hyperbranched polyether, and its molecular weight was 5725g / mol as measured by GPC.

[0190] The above 69.2g of the recovered itaconic acid adduct r-DOPO-IA, 277.5g of epichlorohydrin, 105.6g of ethyl acetate and 0.6g of tetrabutylammonium bromide were mixed uniformly and stirred at 80°C for 4h, and then 60.0g of 40wt% sodium hydroxide aqueous solution was added to continue the reaction at 25°C for 4h. After the reaction was completed, it was filtered, washed with water, and separated. The organic layer was distilled under reduced pressure to obtain a recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA) with an epoxide value of 0.45mol / 100g; 110.5g of the recovered phosphorus-containing itaconic acid epoxy resin (r-DOPO-E IA), 34.5g of glycerol and 0.8g of tetrabutylammonium bromide were mixed uniformly and stirred at 120°C for 4h to obtain a recovered phosphorus-containing itaconic acid hyperbranched epoxy resin (r-IA-EHBP), and its number average molecular weight was 4024g / mol and its epoxide value was 0.14mol by GPC test. l / 100g.

[0191] Recycling of recyclable flame retardant epoxy resin:

[0192] Then, 100.0 g of bisphenol A epoxy resin, 10.0 g of recovered phosphorus-containing itaconic acid hyperbranched epoxy resin and 250.0 g of recovered hexahydrotriazine-terminated mercapto hyperbranched polyether were mixed and cured at 100° C. for 3 h to obtain a recyclable flame-retardant epoxy resin.

[0193] Comparative Example 1

[0194] 100.0 g of DGEBA and 69.9 g of HT-BM were mixed and cured at 100° C. for 3 h to obtain an epoxy resin.

[0195] The cured epoxy resins obtained in the following Examples 1 to 7 and Comparative Example 1 were placed at 25°C for 24 hours and then subjected to performance tests. The tensile properties were measured according to ASTM 3039, the unnotched impact strength was measured according to ASTM D256, the flexural properties were measured according to ASTM D790, the glass transition temperature was measured according to ASTM D2863, and the oxygen index was measured according to ASTM D2863. The test results are shown in Table 1:

[0196] Table 1 Epoxy resin performance test results of each embodiment

[0197]

[0198] As can be seen from Table 1, compared with Example 6 and Example 7, the recyclable flame-retardant epoxy resin prepared by using nitrogen-containing heterocycles and high molecular weight hyperbranched polymers in Examples 1 to 5 has higher strength, toughness, flame retardancy and glass transition temperature. In addition, due to the characteristics of hyperbranched polymers such as high branching and multiple terminal functional groups, the recyclable flame-retardant epoxy resin prepared by the present invention has much higher tensile strength, flexural strength, impact strength and glass transition temperature than the ordinary epoxy resin in Comparative Example 1. The LOI values ​​are also higher than those in Comparative Example 1. Therefore, it can be concluded that the recyclable flame-retardant epoxy resin of the present invention has excellent mechanical properties and good flame retardant effect, and can achieve closed-loop recycling of flame-retardant epoxy resins.

[0199] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a recyclable flame-retardant epoxy resin, characterized in that: Separately preparing a phosphorus-containing itaconic acid hyperbranched epoxy resin and a hexahydro-s-triazine-terminated thiol hyperbranched polyether, and then mixing and curing the bisphenol A epoxy resin, the phosphorus-containing itaconic acid hyperbranched epoxy resin and the hexahydro-s-triazine-terminated thiol hyperbranched polyether to obtain the recyclable flame-retardant epoxy resin; The preparation method of the phosphorus-containing itaconic acid hyperbranched epoxy resin comprises the following steps: S1-1, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, itaconic acid and a first organic solvent are uniformly mixed, and reacted at 40-80° C. for 1-4 hours; after the reaction is completed, the organic solvent is removed to obtain an itaconic acid adduct; S1-2, the itaconic acid adduct, epichlorohydrin, the second organic solvent and the catalyst are mixed evenly, and reacted at 80-120° C. for 1-4 hours; then, an aqueous sodium hydroxide solution is added, and the reaction is continued at 20-40° C. for 2-4 hours; after the reaction is completed, the mixture is filtered, washed with water, and separated, and the organic layer is distilled under reduced pressure to obtain a phosphorus-containing itaconic acid epoxy resin; S1-3, uniformly mixing the phosphorus-containing itaconic acid epoxy resin, the trivalent hydroxy compound and the catalyst, and reacting at 60-120° C. for 1-8 hours to obtain the phosphorus-containing itaconic acid hyperbranched epoxy resin; The preparation method of the hexahydro-s-triazine thiol-terminated hyperbranched polyether comprises the following steps: S2-1, 2-aminobenzenethiol, 30 wt% formaldehyde aqueous solution and a third organic solvent are mixed at 40-80° C. and reacted for 1-5 hours; after the reaction is completed, the mixture is filtered and the precipitate is dried at 40° C. for 4-6 hours to obtain 2,2,2-(1,3,5)-triphenylthiol-s-triazine; S2-2, first dissolving 2,2,2-(1,3,5)-triphenylthiol-s-triazine in a fourth organic solvent, then slowly dropping an alcohol solution of a divinyl monomer into the above solution, and reacting at 0°C-10°C for 1-3h; after the reaction, removing the fourth organic solvent to obtain the hexahydro-s-triazine-terminated thiol hyperbranched polyether; Wherein, in the alcohol solution of divinyl monomer, the mass of divinyl monomer accounts for 10%-30% of the total mass of the solution; The structure of the hexahydro-s-triazine thiol-terminated hyperbranched polyether is shown in general formula (4), general formula (5) or general formula (6): Among them, R4 is represented by In the structural formula of R4, ***** represents the position connected to -S-CH2-; R5 is expressed as In the structural formula of R5, ****** represents the position of connection with -S- or -SH.

2. The method for preparing a recyclable flame-retardant epoxy resin according to claim 1, characterized in that: In the step S1-1, the mass ratio of the 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to the itaconic acid is 216:130; The mass ratio of the 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to the first organic solvent is 1:(1.0-3.0); The first organic solvent is one of xylene, tetrahydrofuran and propylene glycol methyl ether.

3. The method for preparing a recyclable flame-retardant epoxy resin according to claim 1, characterized in that: In step S1-2, the mass of sodium hydroxide in the sodium hydroxide aqueous solution accounts for 10%-40% of the total mass of the solution; The mass ratio of the itaconic acid adduct, the epichlorohydrin, the sodium hydroxide in the sodium hydroxide aqueous solution, and the second organic solvent is 1.0:(2.7-5.3):(0.2-0.5):(1.5-3.0); The second organic solvent is one of ethyl acetate, methyl acetate or n-butyl acetate.

4. The method for preparing a recyclable flame-retardant epoxy resin according to claim 1, characterized in that: In the step S1-3, the mass ratio of the phosphorus-containing itaconic acid epoxy resin, the trivalent hydroxy compound and the catalyst is 1.0:(0.08-0.30):(0.0001-0.001); The trivalent hydroxy compound is one of trimethylolpropane, tris(2-hydroxyethyl)isocyanurate or glycerol; The catalyst is one of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, hexadecyltriethylammonium bromide, benzyltriethylammonium chloride and trioctylmethylammonium chloride.

5. The method for preparing a recyclable flame-retardant epoxy resin according to any one of claims 1 to 4, characterized in that: The structure of the phosphorus-containing itaconic acid hyperbranched epoxy resin is shown in general formula (1), general formula (2) or general formula (3): Among them, R1 is expressed as In the structural formula of R1, * indicates the position of connection with R3; R2 is expressed as In the R2 structure, when R2 is connected to two R3s, ** and *** represent the position of connection to one R3 respectively. When connected, ** indicates the position connected to R3, *** indicates the position connected to The location of the connection; R3 is expressed as **** represents the position of connection with R1 or R2.

6. The method for preparing a recyclable flame-retardant epoxy resin according to claim 1, characterized in that: In the step 2-1, the mass ratio of the 2-aminothiophenol, formaldehyde and the third organic solvent is 1.0:(0.8-1.0):(2.5-3.5); The third organic solvent is one of methanol, ethanol or isopropanol.

7. The method for preparing a recyclable flame-retardant epoxy resin according to claim 1, characterized in that: The divinyl monomer is one of 1,4-cyclohexanedimethanol divinyl ether, diethylene glycol divinyl ether or tri(ethylene glycol) divinyl ether; the fourth organic solvent is one of dichloromethane, tetrahydrofuran or 1,4-dioxane; the alcohol solution of the divinyl monomer is ethanol, methanol or isopropanol solution of the divinyl monomer; The mass ratio of the 2,2,2-(1,3,5)-triphenylthiol-s-triazine, the divinyl monomer and the fourth organic solvent is 1:(0.2-1.2):(0.6-1.4).

8. The method for preparing a recyclable flame-retardant epoxy resin according to claim 1, characterized in that: The curing temperature is 80-120° C., and the curing time is 1-4 hours. The mass ratio of the bisphenol A epoxy resin, the phosphorus-containing itaconic acid hyperbranched epoxy resin, and the hexahydrotriazine-terminated mercapto hyperbranched polyether is 10.0:1.0:14.2-28.

0.

9. A recyclable flame-retardant epoxy resin, characterized in that: The preparation method is described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • A method for preparing a reprocessable, recyclable, dynamically flame-retardant epoxy resin

    CN113754864B

  • A kind of vanillin basic characteristic flame retardant epoxy resin containing fatty amine and preparation method thereof

    CN114409873B

  • Phosphorus-nitrogen containing halogen-free flame-retardant hyperbranched epoxy resin and preparation method thereof

    CN106832219A

  • Degradable sulfur-containing hyperbranched epoxy resin and preparation method thereof

    CN108794726A