A method for producing non-oriented silicon steel with excellent lamination welding performance

Through clean steel smelting, surface oil removal, degreasing and modification treatment, combined with the use of chromium-free environmentally friendly coatings, the welding performance of non-oriented silicon steel has been optimized, solving the problem of poor welding performance in new energy vehicle drive motors, and achieving high efficiency The welding effect and product quality are improved.

CN115679065BActive Publication Date: 2024-10-29武汉钢铁有限公司
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202211294042.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-10-29
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

The welding performance of non-oriented silicon steel laminates used in new energy vehicle drive motors is poor, resulting in problems such as welding bubbles, broken welds, and distorted welds, which affects user processing efficiency and product quality. In addition, the existing technology mainly focuses on magnetic properties and mechanical properties, and has not yet Can effectively improve welding performance.

Method used

The clean steel smelting method is used to control the crown of the hot-rolled plate and the roughness of the cold-rolled plate, and the surface is deoiled, degreased and modified. It uses a chromium-free environmentally friendly coating liquid to control the coating thickness and baking temperature. Through annealing and rolling The coating process is optimized to ensure the improvement of welding performance.

Benefits of technology

It significantly improves the welding performance of non-oriented silicon steel laminations, reduces welding defects, improves coating adhesion and welding stability, and meets the demand for high-efficiency and high-quality products for new energy vehicle drive motors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115679065B_ABST
    Figure CN115679065B_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing non-oriented silicon steel with excellent lamination welding performance. The components and weight percentage contents of molten steel are as follows: C: ≤0.004%, Si: 1.50%-3.50%, Al: 0.40-1.5%, Mn: 0.40-1.50%, P: ≤0.050%, S: ≤0.0025%, N: ≤0.0025%, Sb or Sn or Sb+Sn: ≤0.15%, Cu: ≤0.04%, and the rest are Fe and inevitable impurities; The ingot is hot rolled, coiled, and then cold rolled to the finished thickness after conventional normalization and pickling; after uncoiling and welding, it passes through an alkali spraying device, an alkali brushing device, an electrolytic cleaning device, a high-pressure water spraying device, a water brushing device, a hot water spraying device, an air knife device, and a hot air drying device in sequence to obtain a strip steel with a clean and dry surface; after entering a horizontal continuous annealing furnace, it is roll-coated with a two-roll or three-roll coater, and finally baked and cured, the baking furnace temperature is 350-650°C, the steel plate temperature is 200-350°C, and the baking time is 20-110s.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for producing non-oriented silicon steel. Background Art

[0002] With the development of electrical production, welding, as a process for fixing silicon steel laminations, has replaced traditional methods such as riveting, crimping, and filling, showing obvious advantages. For some motor and electrical products, the welding of core laminations can not only reduce the number of processes and facilitate the mechanization and automation of production, but also has an obvious effect in improving quality. In the production of new energy vehicle drive motors, argon arc TIG welding or laser welding is basically used to fix the silicon steel stator lamination core.

[0003] The arc burning on the silicon steel lamination is relatively unstable, mainly because there is a layer of insulating paint and oil film on the surface of the silicon steel sheet. When the paint and oil are heated to a certain temperature during the welding process, they will evaporate, decompose and burn, thus generating a large amount of gas, which is easy to cause welding bubbles and fractures, and form a wave of air in the welding area, interfering with the protection of the arc area by the shielding gas, endangering the stability of the arc burning, causing the arc to be erratic and the weld to have poor formability. The thicker the coating or the higher the organic solid content, the greater the impact on welding.

[0004] At present, the production of non-oriented silicon steel for new energy vehicle drive motors generally only focuses on how to improve magnetic properties, mechanical properties, and coating properties, and rarely pays attention to the subsequent user processing performance. As for how to improve the welding performance of silicon steel stacking, it is even less mentioned.

[0005] Patents such as CN107723591A, CN106435358A, CN113981329A, CN108570595A, CN111206192A, CN114196887A, CN105950960A, CN107587039A, and CN114107799 A mainly optimize the composition and process design to reduce iron loss, increase magnetic induction and strength, and meet the requirements of new energy vehicle drive motors for the magnetic and mechanical properties of non-oriented silicon steel.

[0006] Patents such as CN109337419A, CN114262547A, CN110240832A, and CN107216764A focus on developing chromium-free, environmentally friendly insulating coatings for non-oriented silicon steel with excellent insulation, adhesion, corrosion resistance, heat resistance, and punching properties, and do not involve the enhancement and improvement of the welding performance of silicon steel laminations.

[0007] Other patents on non-oriented silicon steel are also mostly based on the control of magnetic and mechanical properties. There are no patents that specifically focus on the welding performance of non-oriented silicon steel laminations. However, with the increasingly widespread application of thick coatings and chromium-free environmentally friendly coating products, especially the non-oriented silicon steel with chromium-free environmentally friendly insulation coating on the surface for new energy vehicle drive motors has doubled in recent years. The existing non-oriented silicon steel with chromium-free environmentally friendly coating for new energy vehicle drive motors has poor welding performance of lamination cores due to the thick surface coating and high organic content, especially argon arc welding (TIG welding) is prone to bubbles, broken welds, poor formability and other welding problems, which restricts user processing efficiency and product application. Users have reported more and more welding problems such as bubbles, broken welds, and twisted welds in lamination core welding, which have affected user processing efficiency and product quality, and restricted the large-scale use of environmentally friendly coating products, which need to be solved urgently. Summary of the invention

[0008] In view of the problems of poor welding performance and many welding defects in existing products, the purpose of the present invention is to provide a method for producing non-oriented silicon steel with excellent stacking welding performance, which can achieve the purpose of maintaining the original magnetic and mechanical properties of the product and effectively improving the coating adhesion performance and stacking welding performance of the product through key element control and production process optimization.

[0009] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0010] A method for producing non-oriented silicon steel with excellent lamination welding performance comprises the following steps:

[0011] 1) The clean steel smelting method is adopted for smelting and continuous casting into billets, and the components and weight percentage contents in the molten steel are: C: ≤0.004%, Si: 1.50% to 3.50%, Al: 0.40 to 1.5%, Mn: 0.40 to 1.50%, P: ≤0.050%, S: ≤0.0025%, N: ≤0.0025%, Sb or Sn or Sb+Sn: ≤0.15%, Cu: ≤0.04%, and the rest are Fe and unavoidable impurities;

[0012] 2) heating the continuous casting billet to 1080-1180°C, keeping the temperature for 0.5-1.0h, and then hot rolling, the final rolling temperature is controlled at 800-900°C, and the coiling temperature is 620-670°C;

[0013] 3) After conventional normalization and pickling, cold rolling to the finished thickness;

[0014] 4) After uncoiling and welding, the cold-rolled steel strip is successively passed through an alkali spraying device, an alkali scrubbing device, an electrolytic cleaning device, a high-pressure water spraying device, a water scrubbing device, a hot water spraying device, an air knife device and a hot air drying device to obtain a steel strip with a clean and dry surface;

[0015] 5) Entering into a horizontal continuous annealing furnace, controlling the first stage soaking temperature at 750-950°C, soaking time at 15-30s, annealing atmosphere at a mixture of H2 and N2 or a full N2 humidified atmosphere, H2 ratio at ≤40%, dew point at -10-60°C, modifying the substrate surface, the modified substrate surface is covered with an oxide film, the average thickness of which is in the range of 0.03-0.5μm; controlling the second stage soaking temperature at 900-1000°C, soaking time at 20-45s, annealing atmosphere at a mixture of H2 and N2 or a full N2 dry atmosphere, H2 ratio at ≤50%, and performing recrystallization annealing;

[0016] 6) Use a two-roller or three-roller coating machine for roller coating, and the coating dry film thickness is controlled at 0.3-4.0 μm / side, and the maximum single-side dry film thickness H and the finished strip steel thickness D satisfy the following relationship: H≤D / 150;

[0017] 7) Bake and solidify.

[0018] According to the above scheme, in step 2, the thickness of the hot-rolled plate is controlled at 1.8 to 2.5 mm, and the convexity is controlled to be ≤40 μm.

[0019] According to the above scheme, the surface roughness of the cold-rolled sheet in step 3 is controlled at 0.4-1.0 μm, and the difference between the same sheet is controlled to be ≤7 μm.

[0020] According to the above scheme, the alkali solution for alkali spraying and alkali scrubbing in step 4 is a sodium hydroxide solution with a temperature of 50-80°C, and the weight percentage of sodium hydroxide is 15-30%; the electrolyte temperature is controlled at 50-70°C, and the current intensity passing through the strip is controlled at 2000-3000A; the water temperature for water scrubbing and water rinsing is 55-85°C.

[0021] According to the above scheme, during coating in step 6, the strip temperature is ≤40°C and the coating liquid temperature is ≤25°C.

[0022] According to the above scheme, the coating liquid used in step 6 is an environmentally friendly coating liquid that does not contain chromium, and the organic resin content is ≤35wt%.

[0023] According to the above scheme, in step 7, the baking furnace temperature is 350-650° C., the steel plate temperature is 200-350° C., and the baking time is 20-110 seconds.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] Non-oriented silicon steel for new energy vehicle drive motors, especially high-efficiency and high-grade products, often add grain boundary segregation elements such as Sb or Sn to improve the organizational texture and magnetic properties, but excessive addition can easily cause intergranular oxidation of the stamping section, and impurity elements segregate at the grain boundary to reduce the surface free energy of the substrate, thereby reducing the affinity of the substrate to the coating liquid, and the coating adhesion and stability deteriorate, ultimately leading to poor welding performance. The present invention controls Sb or Sn or Sb+Sn: ≤0.15%.

[0026] The key point of the hot rolling process is to control the convexity of the hot rolled plate to ≤40μm, so as to facilitate the subsequent cold rolling plate shape and plate difference control.

[0027] Improving the surface roughness of the cold-rolled plate can effectively increase the gap between the core laminations, which is beneficial for the gas generated by the thermal decomposition and gasification of the coating during welding to be quickly released from the surrounding area of ​​the weld into the atmosphere, avoiding excessive gas entering the weld molten pool to form welding bubbles, or causing the molten pool to boil and have excessive fluidity, resulting in sag in the weld, discontinuity and distortion of the weld, but the higher the roughness, the greater the resistance to cold rolling deformation, which increases the difficulty of rolling. The surface roughness of the cold-rolled plate of the present invention is controlled at 0.4-1.0μm; the control of the same plate difference is to reduce the height difference in all directions of the laminated core. When the stacking pressure is released after the laminated core is welded, rebound stress will be generated between the laminations. If the heights of the laminations in all directions are inconsistent, there may be excessive local rebound stress. When the stress is greater than the welding strength, the weld is prone to breakage. Combined with the capacity of the rolling mill, the same plate difference of the present invention is controlled to be ≤7μm.

[0028] The ultimate goal of surface degreasing is to obtain a clean and dry strip steel surface, improve the uniformity and adhesion of the coating, and reduce the adverse effects of the coating on welding performance.

[0029] Surface modification of the substrate before the coating process can further effectively improve the surface roughness of the substrate. The increased surface concave and convex points have a surface roughening effect, which can improve the interface bonding force between the coating and the substrate, and is beneficial to the adhesion of the coating. In addition, during the baking film formation process of the thick coating, the inorganic oxide film can partially reflect the heat of the substrate-coating interface back to the coating body, thereby improving the cross-linking and curing degree of the thick coating at the interface. A further beneficial effect is that the addition of organic resin in the coating liquid can be reduced, thereby reducing the impact on welding performance. The present invention controls the average thickness of the oxide film layer on the surface of the modified substrate to be in the range of 0.03 to 0.5 μm. If the oxide film thickness is too thin, the effect is not obvious, and it is easy to cause discontinuity of the film layer, and the uniformity of the coating performance will be affected; if the oxide film is too thick, the magnetic properties of the substrate will deteriorate to an unacceptable level, and the hard and brittle film layer is very unfavorable for subsequent shearing and punching.

[0030] Adding an appropriate amount of resin to the semi-inorganic silicon steel coating liquid can effectively improve the adhesion of the coating to the silicon steel substrate, but on the other hand, the resin is easily decomposed by heat, especially the high heat during welding will cause the resin in the coating around the weld to undergo thermal decomposition and gasification, generating CO, which is decomposed in the molten pool and becomes dissolved C and O. When the molten pool cools and solidifies, CO is regenerated. If the welding speed is too fast, the gas will break through the molten pool, and the molten pool will solidify before being released into the atmosphere, thus forming welding bubbles; if there are too many gases produced by thermal decomposition, the molten pool will boil, the molten liquid will be too fluid, and a wave of air will be formed in the welding area, interfering with the protection of the arc area by the protective gas, endangering the stability of the arc combustion, causing the arc to be erratic, and easily causing the weld to be distorted and poor in formability. At the same time, when the resin content is increased, the content of inorganic salts is also reduced, so that the amount of inorganic salts is insufficient to form a dense and solid glassy film layer with a complete three-dimensional network structure during sintering and solidification, which reduces the corrosion resistance and heat resistance of the coating. Therefore, the resin content in the coating liquid should be controlled within 35%.

[0031] Since organic resins are all thermosetting resins, the strip temperature and the coating liquid temperature during coating should be controlled, otherwise a thermosetting reaction will occur, which will greatly reduce the affinity of the coating liquid to the strip, which is not conducive to the subsequent film-forming reaction and coating quality. The present invention controls the strip temperature during coating to ≤40°C, and the temperature during coating liquid preparation and coating to ≤25°C.

[0032] The thicker the coating, on the one hand, the more resin decomposition and gasification during welding, which is more likely to cause welding bubbles; on the other hand, since a certain stacking pressure is applied during the welding of silicon steel laminations, the thicker the coating, the greater the rebound stress between the silicon steel laminations when the stacking pressure is released after welding, which is more likely to cause weld fracture. Therefore, under the premise of meeting the requirements of insulation, corrosion resistance and stamping performance, the coating should be as thin as possible, and the dry film thickness of the coating of the present invention is controlled at 0.3-4.0 μm / face. At the same time, the smaller the thickness of the silicon steel sheet, the more silicon steel sheets are required to stack into an iron core of the same height, and the higher the coating content per unit volume, which is not conducive to welding. Therefore, in order to obtain good welding performance, the maximum single-sided dry film thickness H and the finished strip thickness D should satisfy the following relationship: H≤D / 150.

[0033] The sintering and curing process of environmentally friendly insulating coatings (taking phosphate coatings as an example) is quite different from that of chromium-containing coatings. The main film-forming substance of the coating, Al(H2PO4)3, is a PO tetrahedral structure, which dehydrates at high temperatures to form aluminum tripolyphosphate and its hydrates. At high temperatures, further dehydration condensation reactions occur to generate aluminum metaphosphate or aluminum polyphosphate by sharing top-angle oxygen atoms. At higher temperatures, further condensation occurs to form a solid and dense polyaluminum metaphosphate glass film layer. The temperature at which phosphate-based non-oriented silicon steel coatings begin to cure is about 220°C, and the complete curing temperature must reach 260°C. At the same time, the curing temperature should be controlled below 350°C and should not exceed 400°C, otherwise the organic resin will be completely decomposed. Therefore, the baking temperature and time must be strictly controlled. If the baking temperature is too low or the time is too short, the curing will be incomplete, the coating will have poor density, be sticky, and have high water absorption, the corrosion resistance will not be fully exerted, and the stability will not be good, which will affect the lamination welding performance; if the baking temperature is too high or the time is too long, the coating may be over-cured, oxidative decomposition will occur, the integrity will be destroyed, and the adhesion and corrosion resistance will be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 : Actual picture of welding quality of non-oriented silicon steel laminated core obtained in Example 1.

[0035] Figure 2 : Actual picture of welding quality of non-oriented silicon steel laminated core obtained in comparative example 2.

[0036] Figure 3 : Actual picture of welding quality of non-oriented silicon steel laminated core obtained in comparative example 3.

[0037] Figure 4 : Actual picture of welding quality of non-oriented silicon steel laminated core obtained in comparative example 7.

[0038] (Please establish a corresponding relationship between the situation in the attached figure and the example or comparative example product.) DETAILED DESCRIPTION

[0039] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0040] The specific implementation method provides a method for producing non-oriented silicon steel with excellent lamination welding performance:

[0041] 1) The clean steel smelting method is adopted for smelting and continuous casting into billets, and the components and weight percentage contents in the molten steel are: C: ≤0.004%, Si: 1.50% to 3.50%, Al: 0.40 to 1.5%, Mn: 0.40 to 1.50%, P: ≤0.050%, S: ≤0.0025%, N: ≤0.0025%, Sb or Sn or Sb+Sn: ≤0.15%, Cu: ≤0.04%, and the rest are Fe and unavoidable impurities;

[0042] 2) The continuous casting billet is heated to 1080-1180°C, kept at this temperature for 0.5-1.0h, and then hot rolled. The final rolling temperature is controlled at 800-900°C, the coiling temperature is controlled at 620-670°C, the thickness of the hot rolled plate is controlled at 1.8-2.5mm, and the convexity is controlled to be ≤40μm;

[0043] 3) After conventional normalization and pickling, the cold-rolled sheet is cold-rolled to the finished thickness, and the surface roughness of the cold-rolled sheet is controlled at 0.4-1.0 μm, and the difference between the same sheet is controlled at ≤7 μm;

[0044] 4) Surface degreasing and degreasing: after uncoiling and welding, the cold-rolled steel strip is successively passed through an alkali spraying device, an alkali scrubbing device, an electrolytic cleaning device, a high-pressure water spraying device, a water scrubbing device, a hot water spraying device, an air knife device and a hot air drying device to obtain a steel strip with a clean and dry surface; the alkali solution for the alkali spraying and alkali scrubbing is a sodium hydroxide solution at a temperature of 50 to 80° C., and the weight percentage of sodium hydroxide is 15 to 30%; the temperature of the electrolyte is controlled at 50 to 70° C., and the current intensity passing through the steel strip is controlled at 2000 to 3000 A; the water temperature for water scrubbing and water rinsing is 55 to 85° C.

[0045] 5) Continuous annealing, using a horizontal continuous annealing furnace, controlling the first stage soaking temperature at 750-950°C, soaking time at 15-30s, annealing atmosphere at a mixture of H2 and N2 or a full N2 humidified atmosphere, H2 ratio at ≤40%, dew point at -10-60°C, modifying the substrate surface, the modified substrate surface is covered with an oxide film, the average thickness of which is in the range of 0.03-0.5μm; controlling the second stage soaking temperature at 900-1000°C, soaking time at 20-45s, annealing atmosphere at a mixture of H2 and N2 or a full N2 dry atmosphere, H2 ratio at ≤50%, and performing recrystallization annealing;

[0046] 6) Coating: the coating liquid is an environmentally friendly coating liquid that does not contain chromium, and the organic resin content is ≤35% by mass percentage. It is roller coated using a two-roller or three-roller coater. The strip temperature during coating is ensured to be ≤40°C, and the temperature during coating liquid preparation and coating is ≤25°C. The coating dry film thickness is controlled at 0.3-4.0μm / side, and the maximum single-side dry film thickness H and the finished strip thickness D satisfy the following relationship: H≤D / 150;

[0047] 7) Baking and curing, the baking furnace temperature is 350-650°C, the steel plate temperature is 200-350°C, and the baking time is 20-110s.

[0048] The specific values ​​of the main parameters in the method for producing non-oriented silicon steel with excellent lamination welding performance of Examples 1-6 are shown in Table 1. The production steps of Comparative Examples 1-9 are the same as those of the Examples, and the specific values ​​of the main parameters are shown in Table 1.

[0049] Table 1

[0050]

[0051] The coating performance and welding performance of the silicon steel strips produced in Examples 1 to 6 and Comparative Examples 1 to 9 were tested, and the results are shown in Table 2. The coating adhesion test conditions are: GB / T 2522-2017, bending diameter 10 mm; the laminated core weldability test conditions are: tungsten inert gas shielded welding (TIG), current value 100A, welding speed 400mm / min, argon gas flow rate 15L / min, lamination pressure 100kg / cm 2 .

[0052] Table 2

[0053]

[0054]

[0055] It can be seen from Tables 1 and 2 that the non-oriented silicon steel produced by the method provided by the present invention has excellent coating adhesion and appearance quality, and the laminated core has good welding performance without obvious welding defects. Figure 1 As shown in the figure; in Comparative Example 1, due to the addition of excessive grain boundary segregation elements, the stamping section is prone to rust, and the coating adhesion is poor. During stamping, the coating is easy to peel off and adhere to the stamping section, thereby causing welding bubbles and broken welds; in Comparative Example 2, due to poor control of hot rolling convexity, the cold rolling difference is too large, and the weld is broken when the stacking pressure is released after the core is stacked and welded. Figure 2 As shown; the cold rolling roughness of comparative example 3 is small, which is not conducive to the release of the gas generated by thermal decomposition of the coating into the atmosphere during lamination welding, and is likely to cause welding bubble defects. Figure 3As shown; in Comparative Example 4, the organic resin content is too high, the thermal decomposition of the coating produces more gas during welding, the weld pool boils, and the molten liquid has too much fluidity, which easily causes welding bubbles and weld distortion defects; in Comparative Examples 5 and 6, due to the high strip temperature or coating liquid temperature during coating, the organic resin undergoes a thermal curing reaction, which reduces the affinity of the coating liquid to the strip, and the film-forming reaction and coating quality are poor, which easily causes broken weld defects; in Comparative Example 7, the dry film of the coating is too thick, the thermal decomposition of the coating produces more gas during welding, the weld pool boils, and the molten liquid has too much fluidity, which causes welding bubbles, weld distortion, and broken weld defects. Figure 4 As shown; in Comparative Example 8, the coating baking temperature is too low, the curing is incomplete, the coating has poor density, is sticky and astringent, has high water absorption, and is prone to welding bubbles and weld bead distortion defects; in Comparative Example 9, the coating baking time is too long, the coating is over-cured, oxidative decomposition occurs, the integrity is destroyed, the adhesion is reduced, and broken weld defects are easily produced.

Claims

1. A method for producing non-oriented silicon steel with excellent lamination welding performance, characterized in that The steps include: 1) The clean steel smelting method is used for smelting and continuous casting into billets. The components and weight percentages in the molten steel are: C: ≤0.004%, Si: 1.50%~3.50%, Al: 0.40~1.5%, Mn: 0.40~1.50%, P: ≤0.050%, S: ≤0.0025%, N: ≤0.0025%, Sb or Sn or Sb+Sn: ≤0.15%, Cu: ≤0.04%, and the rest are Fe and unavoidable impurities; 2) Heat the continuous casting billet to 1080~1180℃, keep it warm for 0.5~1.0h, then hot roll it. The final rolling temperature is controlled at 800~900℃, and the coiling temperature is 620~670℃; 3) After conventional normalization and pickling, cold rolling to the finished thickness; 4) After uncoiling and welding, the cold-rolled steel strip is continuously passed through an alkali spraying device, an alkali brushing device, an electrolytic cleaning device, a high-pressure water spraying device, a water brushing device, a hot water spraying device, an air knife device and a hot air drying device to obtain a steel strip with a clean and dry surface; 5) Enter the horizontal continuous annealing furnace, control the first stage absorptive temperature to 750~950℃, the absorptive time to 15~30s, the annealing atmosphere to be a mixture of H2 and N2 or a full N2 humidified atmosphere, the H2 ratio to be ≤40%, the dew point to be -10~60℃, modify the substrate surface, and the modified substrate surface is covered with an oxide film with an average thickness range of 0.03~0.5μm; control the second stage absorptive temperature to 900~1000℃, the absorptive time to 20~45s, the annealing atmosphere to be a mixture of H2 and N2 or a full N2 dry atmosphere, the H2 ratio to be ≤50%, and perform recrystallization annealing; 6) Use a two-roller or three-roller coater for roller coating, and the coating dry film thickness is controlled at 0.3~4.0μm / side, and the maximum single-side dry film thickness H and the finished strip steel thickness D meet the following relationship: H≤D / 150; 7) Baking and curing, the baking furnace temperature is 350~650℃, the steel plate temperature is 200~350℃, and the baking time is 20~110s.

2. The method for producing non-oriented silicon steel with excellent lamination welding performance as claimed in claim 1, characterized in that In step 2, the thickness of the hot-rolled plate is controlled at 1.8-2.5 mm, and the convexity is controlled at ≤40 μm.

3. The method for producing non-oriented silicon steel with excellent lamination welding performance as claimed in claim 1, characterized in that In step 3, the surface roughness of the cold-rolled sheet is controlled at 0.4-1.0 μm, and the difference between the same sheet and the same sheet is controlled at ≤7 μm.

4. The method for producing non-oriented silicon steel with excellent lamination welding performance as claimed in claim 1, characterized in that In step 4, the alkali solution for alkali spraying and alkali scrubbing is a sodium hydroxide solution at a temperature of 50-80°C, and the weight percentage of sodium hydroxide is 15-30%; the electrolyte temperature is controlled at 50-70°C, and the current intensity passing through the strip is controlled at 2000-3000A; the water temperature for water scrubbing and water rinsing is 55-85°C.

5. The method for producing non-oriented silicon steel with excellent lamination welding performance as claimed in claim 1, characterized in that During step 6 coating, the strip temperature is ≤40°C and the coating liquid temperature is ≤25°C.

6. The method for producing non-oriented silicon steel with excellent lamination welding performance as claimed in claim 1, characterized in that The coating liquid used in step 6 is an environmentally friendly coating liquid that does not contain chromium, and the organic resin content is ≤35wt%.

Citation Information

Patent Citations

  • Non-oriented silicon steel for drive motor of electric automobile and preparation method thereof

    CN105950960A

  • Manufacturing method of high-strength non-oriented silicon steel for new energy vehicle driving motor

    CN106435358A

  • Preparation method of non-oriented silicon steel environment-friendly insulating paint

    CN107216764A

  • Non-oriented silicon steel with excellent magnetism and for drive motor of electric car, and production method thereof

    CN107587039A

  • Cold rolled non-oriented electrical steel for driving motor of new energy automobile and production method thereof