A copper metallographic etching agent and a copper grain boundary etching method and application thereof

Through copper metallographic erosol composed of sulfuric acid, sodium dodecyl sulfonate, water and ethanol, combined with hydrogen peroxide and alcohol polishing technology, the difficulty of copper corrosion agent removing scratches and displaying grain boundaries is solved, achieving high accuracy and Environmentally friendly metallographic inspection avoids the use of 6-valent chromium ions.

CN115679323BActive Publication Date: 2024-11-15SHANGHAI NONFERROUS METALS IND TECH MONITORING CENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202211430945.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-15
Publication Date
2024-11-15
Estimated Expiration
2042-11-15

AI Technical Summary

Technical Problem

Existing copper erosive agents have difficulties in removing scratches and displaying grain boundaries. Conventional agents are prone to over-corrosion or insufficient corrosion, and contain carcinogenic hexavalent chromium ions, resulting in detection errors and environmental pollution problems.

Method used

Using copper metallographic erosol composed of sulfuric acid, sodium dodecyl sulfonate, water and ethanol, hydrogen peroxide is added to improve ionization and oxidation, combined with cross wipe and alcohol polishing technology, remove scratches and reveal clear metallographic Topologies, avoid hexavalent chromium ions.

Benefits of technology

It improves the accuracy and photo clarity of copper metallographic inspection, reduces measurement errors, and the method is environmentally friendly, has simple waste treatment, stable performance, and is easy to store.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003945099360000011
    Figure HDA0003945099360000011
  • Figure HDA0003945099360000012
    Figure HDA0003945099360000012
  • Figure HDA0003945099360000021
    Figure HDA0003945099360000021
Patent Text Reader

Abstract

The present invention belongs to the field of physical and chemical detection technology, and specifically relates to a copper metallographic etchant and a copper grain boundary etchant method and application. The copper metallographic etchant of the present invention is prepared by adding 1-3 parts of hydrogen peroxide to every 100 parts of etchant A, and the etchant A is composed of 5-10 parts of sulfuric acid, 2-3 parts of sodium dodecyl sulfate, 50-60 parts of water, and 30-40 parts of ethanol. The etchant of the present invention can be prepared with tap water, which is easy to obtain and easy to prepare. The etchant of the present invention solves the problems of difficult to remove scratches, severe oxidation of the etched surface, and incomplete display of grain boundaries encountered by the previous etchant, and improves the accuracy of grain size testing; the etchant has stable performance, is easy to store, does not contain hexavalent chromium ions, and is environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of physical and chemical detection, and in particular relates to a copper metallographic etchant and a copper grain boundary etch method and application. Background Art

[0002] The grain size of a material is closely related to its mechanical properties, corrosion resistance, and electrical conductivity. For copper and copper alloys, grain size is one of the important properties that researchers and producers pay attention to. Copper and copper alloys, especially red copper, are easily oxidized, resulting in uneven corrosion of the sample surface, difficulty in removing oxidation spot contamination, blurred grain boundaries, and scratch interference, which leads to large errors in the test results.

[0003] Copper and copper alloys are soft, especially red copper, and scratches on metallographic samples are difficult to remove. Conventional copper and copper alloy etchants, Fe(Cl)3 hydrochloric acid aqueous solution, have strong oxidizing effect and have a certain effect on the display of brass, bronze, and white copper grain boundaries. Red copper with a copper content higher than 90%wt is prone to over-corrosion and oxidation spots, which greatly interfere with the display of grain boundaries and grain size determination. Fe(NO3)3 alcohol solution has weak oxidizing effect, but low ionization degree and weak corrosion effect, resulting in incomplete display of grain boundaries, which is also not conducive to accurate measurement of grain size. Acidic potassium dichromate solution has a good corrosion effect, but contains hexavalent chromium ions, which are easily absorbed by the human body and have strong toxicity and carcinogenicity. On July 23, 2019, it was included in the "Unnamed List of Toxic and Hazardous Water Pollution (First Batch)". Summary of the invention

[0004] The first purpose of the present invention is to provide a copper metallographic etching agent, which can improve the problems of difficult removal of scratches on the copper surface during sample preparation, severe oxidation during etching and incomplete display of grain boundaries, and the water in the etching agent can be selected from tap water, which is easy to obtain and has stable performance.

[0005] The second purpose of the present invention is to provide a method for etching the grain boundaries of copper, which can be used for metallographic inspection of copper, improve the clarity and aesthetics of metallographic photographs, thereby improving the accuracy of detection, reducing measurement errors, and obtaining good display effects.

[0006] The third object of the present invention is to provide an etchant for use in metallographic structure and grain size inspection. The etchant does not contain hexavalent chromium ions, is relatively environmentally friendly, and has simple waste liquid treatment.

[0007] The present invention is achieved through the following technical solutions:

[0008] In a first aspect, the present invention provides a copper metallographic etchant, which is prepared by adding 1-3 parts of hydrogen peroxide to every 100 parts of etchant A; the etchant A is mainly composed of the following reagents in parts by weight: 5-10 parts of sulfuric acid, 2-3 parts of sodium dodecyl sulfate, 50-60 parts of water and 30-40 parts of ethanol.

[0009] Furthermore, in a preferred embodiment of the present invention, the above-mentioned sulfuric acid, sodium dodecyl sulfate, ethanol and hydrogen peroxide are respectively analytically pure or ultra-pure.

[0010] Furthermore, in a preferred embodiment of the present invention, the water is tap water or purified water.

[0011] In a second aspect, the present invention provides a method for etching copper grain boundaries, wherein the copper is cut, inlaid, ground and polished, and then the surface is wiped with a copper metallographic etching agent, and finally metallographic observation is performed.

[0012] Furthermore, in a preferred embodiment of the present invention, the wiping is performed in a cross-pattern for 10 to 50 times.

[0013] Furthermore, in a preferred embodiment of the present invention, the cutting is any one of sawing, shearing and wire cutting.

[0014] Furthermore, in a preferred embodiment of the present invention, the above-mentioned inlay is epoxy resin cold inlay.

[0015] Further, in a preferred embodiment of the present invention, the grinding is manual grinding or automatic grinding, the rotation speed is 300-500rps, and the time is 3-5min. Precautions for the above method: Each grinding step is about 0.5-1min, and each step needs to be rotated 90° to ensure that the cutting scratches are completely removed.

[0016] Furthermore, in a preferred embodiment of the present invention, the polishing is alcohol polishing, with a rotation speed of 500-900rps and a time of 1-2min. Copper is soft, alcohol evaporates faster than water, and the frictional scratch removal effect is stronger, while the deeper polishing scratches caused by diamond polishing paste can be avoided.

[0017] In a third aspect, the present invention provides an application of an etchant in metallographic structure and grain size inspection.

[0018] Compared with the prior art, the present invention has at least the following technical effects:

[0019] The etchant of this scheme can be prepared with tap water, which is easy to obtain and prepare. The etchant of this scheme solves the problems of difficult-to-remove scratches, severe oxidation of the etched surface, and incomplete display of grain boundaries encountered by previous etchants, thereby improving the accuracy of grain size testing. The etchant has stable performance and is easy to store.

[0020] The copper grain boundary erosion method of the present invention can be used for copper metallographic inspection to improve the clarity and aesthetics of metallographic photographs, thereby improving the accuracy of detection, reducing measurement errors, and obtaining a good display effect.

[0021] The etchant of this scheme is used in metallographic structure and grain size inspection. It does not contain hexavalent chromium ions with strong toxicity and carcinogenicity. It can solve the problems of difficult removal of copper oxidation spots, incomplete display of grain boundaries, and difficult removal of scratches, provide metallographic display effects, and reduce test errors. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Example 1: Microscopic diagram of polished state

[0023] Figure 2 Example 1 Microscopic diagram of erosion state

[0024] Figure 3 Example 2: Microscopic diagram of polished state

[0025] Figure 4 Example 2 Microscopic diagram of erosion state

[0026] Figure 5 Example 3: Microscopic diagram of polished state

[0027] Figure 6 Example 3 Microscopic diagram of erosion state

[0028] Figure 7 Comparative Example 1: Microscopic diagram of erosion state

[0029] Figure 8 Comparative Example 2: Microscopic diagram of erosion state DETAILED DESCRIPTION

[0030] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0031] The technical solution of the specific trial method of the present invention is:

[0032] The invention provides a copper metallographic etchant, which is prepared by adding 1-3 parts of hydrogen peroxide to every 100 parts of etchant A; the etchant A mainly consists of the following reagents by weight: 5-10 parts of sulfuric acid, 2-3 parts of sodium dodecyl sulfate, 50-60 parts of water and 30-40 parts of ethanol. The advantage of selecting the above substances is that sulfuric acid has strong ionization and provides sufficient hydrogen ions. Sodium dodecyl sulfate is a surfactant in the etchant formula, and can promote the generation of cuprous oxide and other corrosion products in coordination with sulfuric acid, and then remove the oxidation spots on the eroded surface of the sample to obtain a clear and clean metallographic morphology. The electrode potential of pure copper is relatively high, and the strong oxidizing property of an appropriate amount of hydrogen peroxide increases the electrode potential of the solution and promotes the progress of corrosion. Due to the strong oxidizing property of hydrogen peroxide, the distortion at the grain boundary is relatively high and it is easy to corrode, and the distortion inside the grain is relatively low and it is relatively difficult to corrode. The corrosion inhibition effect of an appropriate amount of ethanol reduces the corrosion effect of the solution on the grain, thereby increasing the display contrast difference between the grain boundary and the grain, and having a better corrosion effect.

[0033] Furthermore, in a preferred embodiment of the present invention, the above-mentioned sulfuric acid, sodium dodecyl sulfate, ethanol and hydrogen peroxide are analytically pure or premium pure, respectively. The above-mentioned substances ensure that impurities are controllable. The strong ionization of sulfuric acid, the surface activity of sodium dodecyl sulfate, the strong oxidizing property of hydrogen peroxide, and the corrosion inhibition of ethanol are coupled with each other, avoiding the strong oxidizing property and the appearance of oxidation spots on the sample surface, and at the same time avoiding the strong corrosive property and the small difference in grain boundary and grain lining, promoting the shedding of corrosion products, and thus obtaining a good display effect.

[0034] Furthermore, in a preferred embodiment of the present invention, the water is tap water or purified water. Generally, purified water is a better choice. Tap water contains a small amount of minerals, but in this solution, sodium dodecyl sulfate is added to promote the shedding of corrosion products to a great extent, avoiding the influence of the precipitation of other unknown minerals in tap water on the corrosion process. In this solution, tap water can be selected, which has a wide source and does not require instrument preparation, saving laboratory costs.

[0035] In a second aspect, the present invention provides a method for etching copper grain boundaries, wherein the copper is cut, inlaid, ground and polished, and then the surface is wiped with a copper metallographic etching agent, and finally metallographic observation is performed.

[0036] Grinding removes enough material to remove areas where the structure has been altered by cutting. Plane or rough grinding can be performed on a belt, a rotating grinding wheel or a stone. In fine grinding, damage to the sample caused by the rough plane grinding step is eliminated. The above metallographic sample preparation process requires grinding to more than 2000 mesh and polishing until there are no obvious coarse scratches.

[0037] Furthermore, in a preferred embodiment of the present invention, the wiping is performed in a cross-pattern for 10 to 50 times. The advantage of the cross-pattern is that polishing scratches and wiping marks can be removed.

[0038] Furthermore, in a preferred embodiment of the present invention, the cutting is any one of sawing, shearing and wire cutting.

[0039] Furthermore, in a preferred embodiment of the present invention, the above-mentioned inlay is epoxy resin cold inlay. The advantage of choosing the cold inlay method is that there is no heating or pressurization, which avoids the stress deformation of the copper during the inlay process.

[0040] Further, in a preferred embodiment of the present invention, the grinding is manual grinding or automatic grinding, the rotation speed is 300-500rps, and the time is 3-5min. Precautions for the above method: Each grinding step is about 0.5-1min, and each step needs to be rotated 90° to ensure that the cutting scratches are completely removed.

[0041] Furthermore, in a preferred embodiment of the present invention, the polishing is performed with analytical pure alcohol at a speed of 500-900 rps for 1-2 min. Copper is soft, alcohol evaporates faster than water, and the frictional scratch removal effect is stronger, while the deeper polishing scratches caused by diamond polishing paste can be avoided.

[0042] In a third aspect, the present invention provides an application of an etchant in metallographic structure and grain size inspection.

[0043] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0044] The reagents used in this protocol, sulfuric acid, sodium dodecyl sulfate, hydrogen peroxide, and ethanol, were purchased from Sinopharm Chemical Reagent Co., Ltd. and were of analytical grade.

[0045] The microscope used in this study was purchased from Zeiss, model Axioscope 7.

[0046] Example 1

[0047] This embodiment provides a copper metallographic etching agent:

[0048] Etching agent A is composed of 5 ml of analytical grade sulfuric acid, 2 g of analytical grade sodium dodecyl sulfate, 55 ml of water, and 30 ml of analytical grade ethanol;

[0049] Select 100 ml of etchant A and add 1 ml of hydrogen peroxide to prepare etchant 1.

[0050] This embodiment provides a method for etching copper grain boundaries:

[0051] Cutting: The material is copper tube for air conditioner, brand TU0, diameter 15mm, wall thickness 1mm. Use tube cutter to cut samples with diameter 15mm, wall thickness 1mm and length 15mm.

[0052] Mounting: Cold mounting with epoxy resin: Place the sample in a plastic mold and then pour the resin around the sample. There should be no gap between the sample surface and the mounting material to prevent the corrosive agent from leaking out before the evaluation is completed.

[0053] Grinding: Grind the specimens with 120, 240, 500, 1000, 2000, 3000 grit sandpaper respectively, ensuring that the sandpaper or cutting and processing marks are completely removed. The minimum material removal of the sample is 0.5mm, and the processing marks are removed. After all grinding is completed, the sample must be thoroughly cleaned. The speed of manual grinding is 500rps and the grinding time is 5min.

[0054] Polishing: Use alcohol for polishing. Store the alcohol in a pointed squeeze pot and spray for about 1 second each time. Add about 1-5ml of alcohol each time and spray once every 10-15 seconds. The manual polishing speed is 900rps and polishing takes 1min.

[0055] Corrosion: Use corrosive agent 1, soak it with a cotton ball, wipe it 15 times with a cross, and observe it under a metallographic microscope.

[0056] Polished state Figure 1 , there are a few polishing marks; see the erosion state picture Figure 2 After being wiped with copper etching agent, the interface is clear and no traces are seen.

[0057] Example 2

[0058] Etching agent A is composed of 8 ml of sulfuric acid, 3 g of sodium dodecyl sulfate, 50 ml of water, and 40 ml of ethanol.

[0059] Select 100 ml of etchant A and add 3 parts of hydrogen peroxide to prepare etchant 2.

[0060] This embodiment provides a method for etching copper grain boundaries:

[0061] The material is copper tube for air conditioning, brand TU0, diameter 15mm, wall thickness 1.0mm. A tube cutter is used to cut a sample of about 15mm in length, and epoxy resin is used for cold mounting.

[0062] Mounting: Cold mounting with epoxy resin: Place the sample in a plastic mold and then pour the resin around the sample. There should be no gap between the sample surface and the mounting material to prevent the corrosive agent from leaking out before the evaluation is completed.

[0063] Grinding: Grind the specimens with 120, 240, 500, 1000, 2000, 3000 grit sandpaper respectively, ensuring that the sandpaper or cutting and processing marks are completely removed. The minimum material removal of the sample is 0.5mm, and the processing marks are removed. After all grinding is completed, the sample must be thoroughly cleaned. The speed of manual grinding is 400rps and the grinding time is 3min.

[0064] Polishing: Use alcohol for polishing. Store the alcohol in a pointed squeeze pot and spray for about 1 second each time. Add about 1-5ml of alcohol each time and spray once every 10-15 seconds. The manual polishing speed is 800rps and polishing takes 1min.

[0065] Use etchant 2, soak a cotton ball, rub 50 times with a cross, and observe under a metallographic microscope.

[0066] Polished state Figure 3 , there are a few polishing marks; see the erosion state picture Figure 4 After being wiped with copper etching agent, the interface is clear and no traces are seen.

[0067] Example 3

[0068] Etching agent A is composed of 7 ml of sulfuric acid, 3 g of sodium dodecyl sulfate, 55 ml of water, and 35 ml of ethanol.

[0069] Select 100 ml of etching agent A and add 2 parts of hydrogen peroxide to prepare etching agent 3.

[0070] This embodiment provides a method for etching copper grain boundaries:

[0071] The material is a copper tube for air conditioning, brand TP2, diameter 10 mm, wall thickness 0.8 mm, a tube cutter is used to cut a sample of about 15 mm in length, and epoxy resin is used for cold mounting. The grinding and polishing method in Example 1 is used to prepare the sample.

[0072] Mounting: Cold mounting with epoxy resin: Place the sample in a plastic mold and then pour the resin around the sample. There should be no gap between the sample surface and the mounting material to prevent the corrosive agent from leaking out before the evaluation is completed.

[0073] Grinding: Use an automatic grinder (ATM QPOI 250A2) to grind the specimens with 120, 240, 500, 1000, 2000, and 3000 grit sandpapers, respectively. Set the grinding time for each step to 40s, a total of 240s, and a speed of 300rps to ensure that the sandpaper or cutting and processing marks are completely removed. The minimum material removal of the sample is 0.5mm to remove the processing marks. After all grinding is completed, the sample must be thoroughly cleaned.

[0074] Polishing: Use an automatic grinder (ATM QPOI 250A2) and polish with alcohol. Store the alcohol in a pointed squeeze pot and spray for about 1 second each time. Add about 1-5ml of alcohol each time, spray once every 10-15 seconds, set the speed to 500rps, and polish for 2 minutes.

[0075] Use etching agent 3, soak it with a cotton ball, rub it 40 times with a cross, and observe it under a metallographic microscope.

[0076] Polished state Figure 5 , there are a few polishing marks; see the erosion state picture Figure 6 After being wiped with copper etching agent, the interface is clear and no traces are seen.

[0077] Comparative Example 1

[0078] The etching agent of the comparative example is composed of 5 g of ferric chloride hexahydrate, 10 ml of hydrochloric acid and 90 ml of water.

[0079] The comparative example of the copper grain boundary etching method adopts the sample preparation and etching steps of Example 1, and the microscopic effect diagram is as follows: Figure 7 There are relatively more oxidation spots, the solution is highly corrosive, the grain boundaries within the crystal are deeply corroded, and the contrast difference is small.

[0080] Comparative Example 2

[0081] The etching agent of the comparative example is composed of 20 g of ferric nitrate nonahydrate and 100 ml of ethanol (ferric nitrate saturated alcohol solution).

[0082] The comparative example of the copper grain boundary etching method adopts the sample preparation and etching steps of Example 1, and the microscopic effect diagram is as follows: Figure 8 There are fewer oxidation spots, but the corrosion is weaker, and there is little difference in intragranular and intergranular corrosion.

[0083] In the above-mentioned Examples 1-3, there are a few polishing marks in the polishing image, and in the etched image, the interface after wiping with the copper etchant is clear and no marks are seen.

[0084] However, in the erosion diagram of comparative example 1, there are relatively more oxidation spots, the solution is highly corrosive, the grain boundaries within the crystal are deeply corroded, and the contrast difference is small. Although there are fewer oxidation spots in the erosion diagram of comparative example 2, the corrosion is weaker, and the difference in grain boundary corrosion within the crystal is not significant.

[0085] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A copper metallographic etching agent, characterized in that: The etchant is prepared by adding 1-3 parts by volume of hydrogen peroxide to every 100 parts by volume of etchant A; The etching agent A is mainly composed of the following reagents in parts by weight: Composition: 5-10 parts of sulfuric acid, 2-3 parts of sodium dodecyl sulfate, 50-60 parts of water and 30-40 parts of ethanol.

2. The etching agent according to claim 1, characterized in that The sulfuric acid, sodium dodecyl sulfate, ethanol and hydrogen peroxide are of analytical grade.

3. The etching agent according to claim 1, characterized in that The water is tap water or purified water.

4. A method for etching copper grain boundaries, characterized in that: After the copper is cut, inlaid, ground and polished, the surface is wiped with the etching agent described in any one of claims 1 to 3, and finally metallographic observation is performed.

5. The method for etching copper grain boundaries according to claim 4, characterized in that: The wiping is performed by cross wiping, and the wiping is performed 10-50 times.

6. The method for etching copper grain boundaries according to claim 4, characterized in that: The cutting is any one of sawing, shearing and wire cutting.

7. The method for etching copper grain boundaries according to claim 4, characterized in that: The inlay is epoxy resin cold inlay.

8. The method for etching copper grain boundaries according to claim 4, characterized in that: The grinding is manual grinding or automatic grinding, with a rotation speed of 300-500 rps and a time of 3-5 min.

9. The method for etching copper grain boundaries according to claim 4, characterized in that: The polishing is alcohol polishing, with a rotation speed of 500-900rps and a time of 1-2min.

10. Use of the etchant according to any one of claims 1 to 3 in metallographic structure and grain size inspection.

Citation Information

Patent Citations

  • Corrosion method for small-specification red copper rod

    CN105177577A

  • Method for metallographic corrosion of large-size copper bar

    CN105181428A

  • Corrosive agent for displaying grain boundaries of high-damping manganese-based copper alloys and corrosion method thereof

    CN106404502A

  • Metallographic pregrinding machine capable of automatically cutting and replacing abrasive paper

    CN213615914U

  • Corrosion resistance testing method for copper-based member

    JP2012215410A