A method for preparing polyester filaments

By depositing a titanium dioxide film on the surface of coconut carbon fiber and combining it with composite functional additives in melt spinning technology, the problems of insufficient warmth retention and limited color of polyester long fiber have been solved, achieving multi-color, warmth retention and antibacterial effects for polyester long fiber.

CN115679473BActive Publication Date: 2024-11-15XINJIANG JINDAYU ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211441114.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-17
Publication Date
2024-11-15
Estimated Expiration
2042-11-17

AI Technical Summary

Technical Problem

The existing polyester filament has insufficient thermal insulation properties to meet the needs of warmth, and the color of coconut charcoal fiber limits its application range.

Method used

Polyester long fibers were prepared by depositing a titanium dioxide film on the surface of coconut carbon fiber ultrafine powder, adding a specific amount of coconut carbon fiber powder with titanium dioxide film and composite functional additives to the polyester chip system, and combining it with melt spinning technology.

Benefits of technology

The prepared polyester filaments possess excellent warmth retention, dryness and comfort, and antibacterial properties, while also being able to display a variety of colors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003948416970000081
    Figure BDA0003948416970000081
  • Figure BDA0003948416970000091
    Figure BDA0003948416970000091
Patent Text Reader

Abstract

The invention relates to a method for preparing polyester filaments; the composite functional additive is a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, which can enable the polyester staple fiber to obtain good far-infrared emission function, thereby obtaining good thermal insulation performance, and can be combined with the design of powder particle size to further improve its thermal insulation performance; and the mineral content in coconut charcoal is various. Coconut charcoal can absorb and emit far-infrared rays with a wavelength of 4 to 14 μm, thereby stimulating the formation of negative ions that are beneficial to the body, and because the other raw materials of the polyester staple fiber have thermal insulation performance, combined with coconut charcoal fiber, a porous and water-permeable surface layer can be generated on the fiber surface, which can dissolve skin sweat and quickly diffuse and evaporate, ensuring dryness and comfort while keeping warm and avoiding bacterial growth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of spinning, and in particular to a method for preparing polyester filaments. Background Art

[0002] Polyester filaments are made of polyester. Polyester is an important variety of synthetic fibers and is the trade name of polyester fibers in my country. It is a fiber-forming polymer made of polyethylene terephthalate (PET) through esterification or ester exchange and polycondensation reaction with purified terephthalic acid (PTA) or dimethyl terephthalate (DMT) and ethylene glycol (MEG) as raw materials, and is made of polyethylene terephthalate (PET) through spinning and post-treatment. Polyester fibers are divided into two types: long fibers and short fibers. The so-called polyester filaments are filaments with a length of more than one kilometer, and the long fibers are wound into balls. Polyester staple fibers are short fibers ranging from a few centimeters to more than ten centimeters. Polyester filaments can be divided into: primary silk (including unstretched silk, semi-pre-oriented silk, pre-oriented silk, highly oriented silk), drawn silk (drawn silk, fully drawn silk, fully taken silk), and deformed silk (conventional deformed silk, drawn deformed silk and air-deformed silk) according to their uses. They are mainly divided into civil and industrial silk.

[0003] A Chinese patent application numbered CN201810903883.5 discloses a polyester filament and a method for preparing the same. The method has the advantages of avoiding the occurrence of lint and breakage in the spinning process and being easy to prepare.

[0004] However, the thermal insulation performance of existing polyester filaments is difficult to meet the thermal insulation needs.

[0005] Coconut charcoal fiber is a new type of environmentally friendly material. When the coconut pulp and coconut water are taken away and processed into food, the coarse coconut shell waste will cause great pressure on environmental remediation. However, people collect the waste coconut shells and make them recyclable. Through soaking, beating, filtering residues, and drying, we can finally obtain the fiber of coconut shells: coconut fiber. Then, the coconut fiber is heated to 1200℃ and carbonized at high temperature to obtain coconut charcoal with excellent properties. The molecular formula of coconut charcoal is hexagonal, the carbon is inseparable, the relative density is large, and there are many pores. The total area of ​​the microporous plate is more than 4 times that of bamboo charcoal, and it has a strong adsorption function.

[0006] In the prior art, although there are publicized recipes for using coconut charcoal fiber as fabrics, for example, a Chinese patent with authorization announcement number CN106435944B discloses a new type of antibacterial fabric, and its specific preparation method is to add pearl fiber; wool fiber; corn protein fiber; modal fiber; coconut charcoal fiber; tea fiber; antibacterial finishing agent at 40-45°C, add dispersant, binder, softener, add 100-120 parts of water, mix and stir evenly, and then air-dry to form; then the mixture is subjected to cleaning, opening, drawing, coarse yarn, and spun yarn to form functional yarn lines; and then the functional yarn lines are knitted or woven into cloth. It can be seen that in the prior art, carbon fiber is mixed with other fiber materials and then made into yarn according to the traditional spinning process of cleaning, opening, drawing, roving and spinning, and is not combined with the melt spinning technology of polyester fiber. Since the color of coconut charcoal fiber itself is dark black and its dyeing performance is poor, the yarn or fabric using coconut charcoal fiber on the market is gray-black in color, thus limiting the scope of use.

[0007] Based on the above-mentioned existing technology, there is an urgent need to provide a method for preparing polyester filaments, so that the prepared polyester filaments have the advantages of warmth, dryness, comfort and antibacterial, and can also make the prepared polyester filaments have more diverse colors. Summary of the invention

[0008] The technical problem to be solved by the present invention is: it is urgent to provide a method for preparing polyester filaments, so that the prepared polyester filaments have the advantages of warmth retention, dryness and comfort, and antibacterial, and can also make the prepared polyester filaments have more diverse colors.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0010] A method for preparing polyester filaments comprises the following steps:

[0011] Step 1: preparing superfine coconut charcoal fiber powder;

[0012] Step 2: Place the coconut charcoal fiber ultrafine powder into the reaction vessel of the atomic deposition equipment at a reaction temperature of 100-110°C;

[0013] Step 3: introducing titanium tetraisopropoxide vapor into a continuously stirred reaction vessel for 8 seconds, purging with nitrogen for 20 seconds, and then intermittently introducing deionized water into the reaction vessel for 8 seconds, purging with nitrogen for 20 seconds;

[0014] Repeat the above step 3 for n times, where n is any value between 5 and 10000, to deposit a titanium dioxide film on the surface of the coconut charcoal fiber ultrafine powder;

[0015] Step 4: pre-crystallize the polyester chips with hot air at 130-135°C for 20-30 minutes, and then sequentially perform the first drying and the second drying on the pre-crystallized polyester chips. The first drying temperature is 160-165°C for 15-25 minutes, and the second drying temperature is 150-155°C for 5-8 hours.

[0016] Step 5: 300 parts by weight of the dried polyester chips and 60-0.005 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3; then add 5-10 parts by weight of a composite functional additive, then heat to 200-250° C., and react for 10-15 minutes under a vacuum condition of 200-300 Pa; then add 90-0.007 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3, and then react for 5-10 minutes under a vacuum condition of 230-260° C. and 250-350 Pa to obtain a melt; the composite functional additive is a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, and the mass ratios of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder are 1:(2-4):1:(2-4) in sequence;

[0017] Step 6: melt-spinning the melt to obtain a melt, wherein the spinning temperature is 270-290° C.;

[0018] Step 7: Extruding the melt through a special-shaped spinneret to form a melt stream, cooling it, and solidifying it into a primary silk fiber, wherein the spinneret micropores are in the shape of a gear;

[0019] Step 8: After the spun silk fiber is oiled, it is curled and formed by a winding machine to obtain polyester filaments.

[0020] Furthermore, in the above-mentioned method for preparing polyester filaments, step 4 is specifically as follows: pre-crystallizing the polyester chips with hot air at 132-133°C, the pre-crystallization time is 23-26 min, the first drying temperature is 163-164°C, the first drying time is 21-22 min, the second drying temperature is 152-153°C, and the second drying time is 6.5-7.5 h.

[0021] Furthermore, in the above-mentioned method for preparing polyester filaments, the step 1 is specifically: heating the coconut shell fiber to 1200° C., carbonizing it under a vacuum environment, and ultrafinely grinding the carbonized fiber to obtain coconut charcoal fiber ultrafine powder.

[0022] Furthermore, in the above-mentioned method for preparing polyester filaments, the particle size of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 10-30 microns.

[0023] Furthermore, in the above-mentioned method for preparing polyester filaments, the number of gear-shaped teeth of the spinning microholes of the spinneret is 6-8.

[0024] Furthermore, in the above-mentioned method for preparing polyester filaments, the diameter of the gear-shaped spinning micropores of the spinneret is 0.7-0.8 mm, and the gear-shaped tooth height is 0.15-0.2 mm.

[0025] Furthermore, in the above-mentioned method for preparing polyester filaments, the cooling in step 7 is specifically: using a side-blowing cooling process to solidify into filaments; the conditions of the side-blowing cooling process are: the side-blowing speed is 0.4m / s, the side-blowing temperature is 20°C, and the side-blowing humidity is 70%.

[0026] Furthermore, in the above-mentioned method for preparing polyester filaments, in step 8, the temperature is 24-28° C. and the relative humidity is 45-65%.

[0027] Further, in the above-mentioned method for preparing polyester filaments, the step 5 is specifically as follows: 300 parts by weight of the dried polyester chips and 60-0.005 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3; then 10-15 parts of the masterbatch are added, and then 5-10 parts by weight of the composite functional additive are added, and then the temperature is raised to 200-250°C, and the reaction is carried out under a vacuum condition of 200-300Pa for 10-15min; then 90-0.007 parts by weight of the step The carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3 is then added with 10-15 parts of masterbatch, and then reacted for 5-10 minutes at 230-260° C. and 250-350 Pa vacuum conditions to obtain a melt; the composite functional additive is a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, and the mass ratios of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder are 1:(2-4):1:(2-4) in sequence;

[0028] The present invention also relates to polyester filaments prepared by the method for preparing the polyester filaments.

[0029] The beneficial effects of the present invention are:

[0030] The method of preparing coconut charcoal fiber ultrafine powder and depositing titanium tetraisopropoxide on the surface of coconut charcoal fiber ultrafine powder makes titanium dioxide film uniformly deposited on the surface of coconut charcoal fiber ultrafine powder. This is to utilize the oxygen-containing functional groups such as -OH and -COOH on the surface of coconut charcoal fiber to effectively start the growth characteristics of titanium dioxide film. First, titanium tetraisopropoxide is introduced to form -OCH(CH3)2 on the surface of coconut charcoal fiber through the self-limiting chemical reaction of the active groups of the oxygen-containing functional groups on the surface of coconut charcoal fiber, and H2O is introduced to react with -OCH(CH3)2 to form a single-layer titanium dioxide film and exposed -OH. After each step, the remaining substances are blown away by nitrogen. The required titanium dioxide film thickness can be adjusted by repeating the number of cycles;

[0031] By adjusting the thickness of the titanium dioxide film, the surface of the coconut charcoal fiber can present different colors. In the melt extrusion spinning process, by adding a specific amount of coconut charcoal fiber powder with a titanium dioxide film to the polyester chip system for the second time, the coconut charcoal fiber powder and the polymer can be mixed more evenly, so that when the melt is extruded to form a melt stream, the coconut charcoal fiber can be evenly distributed; in the polyester chip system, according to the color of the coconut charcoal fiber powder, the same color masterbatch is added to make the extruded melt stream present a uniform color;

[0032] The composite functional additive is designed to be a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, and the above mass ratio is designed, so that the polyester staple fiber can obtain good far-infrared emission function, thereby obtaining good thermal insulation performance, and can be combined with the design of powder particle size to further improve its thermal insulation performance; and the mineral content in coconut charcoal is diverse. Coconut charcoal can absorb and emit far-infrared rays with a wavelength of 4 to 14 μm, thereby stimulating the formation of negative ions that are beneficial to the body. In addition, since the other raw materials of the above polyester staple fiber have thermal insulation properties, combined with coconut charcoal fiber, a porous and water-permeable surface layer can be produced on the fiber surface, which can dissolve skin sweat and quickly diffuse and evaporate, ensuring dryness and comfort while keeping warm and avoiding bacterial growth. DETAILED DESCRIPTION

[0033] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in conjunction with the implementation modes.

[0034] Example 1

[0035] A method for preparing polyester filaments comprises the following steps:

[0036] Step 1: heating the coconut shell fiber to 1200°C, carbonizing it under vacuum, and ultrafine grinding the carbonized fiber to obtain coconut charcoal fiber ultrafine powder;

[0037] Step 2: Place the coconut charcoal fiber ultrafine powder into the reaction vessel of the atomic deposition equipment at a reaction temperature of 100-110°C;

[0038] Step 3: introducing titanium tetraisopropoxide vapor into a continuously stirred reaction vessel for 8 seconds, purging with nitrogen for 20 seconds, and then intermittently introducing deionized water into the reaction vessel for 8 seconds, purging with nitrogen for 20 seconds;

[0039] Repeat the above step 3 for 800 times, so that a titanium dioxide film with a thickness of 80nm is deposited on the surface of the coconut charcoal fiber superfine powder, making the coconut charcoal fiber superfine powder appear blue;

[0040] Step 4: pre-crystallize the polyester chips with hot air at 132°C for 24 minutes, the first drying temperature is 163°C for 21 minutes, the second drying temperature is 152°C for 7 hours;

[0041] Step 5: 300 parts by weight of the dried polyester chips and 56 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3; then add 12 parts of blue masterbatch, then add 7 parts by weight of the composite functional additive, then heat to 220°C, and react for 12 minutes under 250Pa vacuum conditions; then add 84.4 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3, then add 10-15 parts of the masterbatch, and then react for 7 minutes under 240°C and 300Pa vacuum conditions to obtain a melt; the composite functional additive is a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, and the mass ratio of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 1:3:1:3 respectively; the particle size of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 20 microns;

[0042] Step 6: melt-spinning the melt to obtain a melt, wherein the spinning temperature is 280° C.;

[0043] Step 7: Extruding the melt through a special-shaped spinneret to form a melt stream, cooling it, and solidifying it into primary silk fibers, and solidifying it into filaments by a side-blowing cooling process; the conditions of the side-blowing cooling process are: the side-blowing speed is 0.4 m / s, the side-blowing temperature is 20° C., and the side-blowing humidity is 70%; the spinneret micropores of the spinneret are in the shape of a gear; the number of teeth of the gear-shaped spinneret micropores of the spinneret is 7; the diameter of the gear-shaped spinneret micropores of the spinneret is 0.7 mm, and the gear-shaped tooth height is 0.17 mm;

[0044] Step 8: After the spun silk fibers are oiled, they are curled on a winding machine at a temperature of 26° C. and a relative humidity of 55% to obtain polyester filaments.

[0045] Example 2

[0046] A method for preparing polyester filaments comprises the following steps:

[0047] Step 1: heating the coconut shell fiber to 1200°C, carbonizing it under vacuum, and ultrafine grinding the carbonized fiber to obtain coconut charcoal fiber ultrafine powder;

[0048] Step 2: Place the coconut charcoal fiber ultrafine powder into the reaction vessel of the atomic deposition equipment at a reaction temperature of 100°C;

[0049] Step 3: introducing titanium tetraisopropoxide vapor into a continuously stirred reaction vessel for 8 seconds, purging with nitrogen for 20 seconds, and then intermittently introducing deionized water into the reaction vessel for 8 seconds, purging with nitrogen for 20 seconds;

[0050] Repeat the above step 3 for 1200 times to deposit a titanium dioxide film with a thickness of 120 nm on the surface of the coconut charcoal fiber superfine powder, so that the coconut charcoal fiber superfine powder appears light blue;

[0051] Step 4: pre-crystallize the polyester chips with hot air at 132°C for 23 minutes, the first drying temperature is 163°C for 21 minutes, the second drying temperature is 152°C for 6.5 hours;

[0052] Step 5: 300 parts by weight of the dried polyester chips and 54 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3; then add 10 parts of light blue masterbatch, then add 5 parts by weight of the composite functional additive, then heat to 200°C, and react for 10 minutes under a vacuum condition of 200Pa; then add 81.6 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3, then add 10 parts of the masterbatch, and then react for 5 minutes under a vacuum condition of 230°C and 250Pa to obtain a melt; the composite functional additive is a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, and the mass ratio of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 1:2:1:2 respectively; the particle size of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 10 microns;

[0053] Step 6: melt-spinning the melt to obtain a melt, wherein the spinning temperature is 270° C.;

[0054] Step 7: Extruding the melt through a special-shaped spinneret to form a melt stream, cooling it, and solidifying it into primary silk fibers, and solidifying it into filaments by a side-blowing cooling process; the conditions of the side-blowing cooling process are: the side-blowing speed is 0.4 m / s, the side-blowing temperature is 20° C., and the side-blowing humidity is 70%; the spinneret micropores of the spinneret are in the shape of a gear; the number of teeth of the gear-shaped spinneret micropores of the spinneret is 6; the diameter of the gear-shaped spinneret micropores of the spinneret is 0.7 mm, and the gear-shaped tooth height is 0.15 mm;

[0055] Step 8: After the spun silk fibers are oiled, they are curled on a winding machine at a temperature of 24° C. and a relative humidity of 45% to obtain polyester filaments.

[0056] Example 3

[0057] A method for preparing polyester filaments comprises the following steps:

[0058] Step 1: heating the coconut shell fiber to 1200°C, carbonizing it under vacuum, and ultrafine grinding the carbonized fiber to obtain coconut charcoal fiber ultrafine powder;

[0059] Step 2: Place the coconut charcoal fiber ultrafine powder into the reaction vessel of the atomic deposition equipment at a reaction temperature of 110°C;

[0060] Step 3: introducing titanium tetraisopropoxide vapor into a continuously stirred reaction vessel for 8 seconds, purging with nitrogen for 20 seconds, and then intermittently introducing deionized water into the reaction vessel for 8 seconds, purging with nitrogen for 20 seconds;

[0061] Repeat the above step 3 for 1600 times to deposit a titanium dioxide film with a thickness of 160 nm on the surface of the coconut charcoal fiber superfine powder, so that the coconut charcoal fiber superfine powder appears golden yellow;

[0062] Step 4: Pre-crystallize the polyester chips with hot air at 133°C, the pre-crystallization time is 26 minutes, the first drying temperature is 164°C, the first drying time is 22 minutes, the second drying temperature is 153°C, and the second drying time is 7.5 hours;

[0063] Step 5: 300 parts by weight of the dried polyester chips and 52 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3; then add 15 parts of golden masterbatch, then add 10 parts by weight of the composite functional additive, then heat to 250°C, and react for 15 minutes under 300Pa vacuum conditions; then add 78.8 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3, then add 15 parts of the masterbatch, and then react for 10 minutes under 260°C and 350Pa vacuum conditions to obtain a melt; the composite functional additive is a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, and the mass ratios of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder are 1:4:1:4 respectively; the particle size of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 30 microns;

[0064] Step 6: melt-spinning the melt to obtain a melt, wherein the spinning temperature is 290° C.;

[0065] Step 7: Extruding the melt through a special-shaped spinneret to form a melt stream, cooling it, and solidifying it into primary silk fibers, and solidifying it into filaments by a side-blowing cooling process; the conditions of the side-blowing cooling process are: the side-blowing speed is 0.4 m / s, the side-blowing temperature is 20° C., and the side-blowing humidity is 70%; the spinneret micropores of the spinneret are in the shape of a gear; the number of teeth of the gear-shaped spinneret micropores of the spinneret is 8; the diameter of the gear-shaped spinneret micropores of the spinneret is 0.8 mm, and the gear-shaped tooth height is 0.2 mm;

[0066] Step 8: After the spun silk fibers are oiled, they are curled on a winding machine at a temperature of 28° C. and a relative humidity of 65% to obtain polyester filaments.

[0067] Performance Test:

[0068] 1. According to GB / T6503-2008, the breaking strength and moisture regain of the polyester filaments obtained in Examples 1 to 3 were tested respectively. The test results are shown in Table 1;

[0069] Table 1

[0070]

[0071]

[0072] According to Table 1, the breaking strength and moisture regain of the polyester filaments obtained in Examples 1 to 3 all meet the standard requirements.

[0073] 2. The polyester filaments obtained in Examples 1 to 3 were spun into fabrics respectively, and then far-infrared performance tests were performed respectively. The test results are shown in Table 2.

[0074] Table 2

[0075] Test groups Normal emissivity Standard requirements for normal emissivity in conclusion Example 1 0.91 ≥0.80 qualified Example 2 0.90 ≥0.80 qualified Example 3 0.89 ≥0.80 qualified

[0076] According to Table 2, the normal emissivity of the fabrics spun from polyester filaments obtained in Examples 1 to 3 is greater than the standard requirement and has a warm-keeping function.

[0077] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing polyester filaments, characterized in that: The following steps are involved: Step 1: heating the coconut shell fiber to 1200°C, carbonizing it under vacuum, and ultrafine grinding the carbonized fiber to obtain coconut charcoal fiber ultrafine powder; Step 2: Place the coconut charcoal fiber ultrafine powder into the reaction vessel of the atomic deposition equipment at a reaction temperature of 100-110°C; Step 3: introducing titanium tetraisopropoxide vapor into a continuously stirred reaction vessel for 8 seconds, purging with nitrogen for 20 seconds, and then intermittently introducing deionized water into the reaction vessel for 8 seconds, purging with nitrogen for 20 seconds; Repeat the above step 3 for 800 times, so that a titanium dioxide film with a thickness of 80nm is deposited on the surface of the coconut charcoal fiber superfine powder, making the coconut charcoal fiber superfine powder appear blue; Step 4: pre-crystallize the polyester chips with hot air at 132°C for 24 minutes, the first drying temperature is 163°C for 21 minutes, the second drying temperature is 152°C for 7 hours; Step 5: 300 parts by weight of the dried polyester chips and 56 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3; then add 12 parts of blue masterbatch, then add 7 parts by weight of the composite functional additive, then heat to 220°C, and react for 12 minutes under 250Pa vacuum conditions; then add 84.4 parts by weight of the carbon fiber ultrafine powder with a titanium dioxide film deposited on the surface obtained in step 3, then add 10-15 parts of the masterbatch, and then react for 7 minutes under 240°C and 300Pa vacuum conditions to obtain a melt; the composite functional additive is a mixture of silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder, and the mass ratio of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 1:3:1:3 respectively; the particle size of the silicon dioxide, germanium dioxide, aluminum oxide and surface-modified aluminum-doped zinc oxide powder is 20 microns; Step 6: melt-spinning the melt to obtain a melt, wherein the spinning temperature is 280° C.; Step 7: Extruding the melt through a special-shaped spinneret to form a melt stream, cooling it, and solidifying it into primary silk fibers, and solidifying it into filaments by a side-blowing cooling process; the conditions of the side-blowing cooling process are: the side-blowing speed is 0.4 m / s, the side-blowing temperature is 20° C., and the side-blowing humidity is 70%; the spinneret micropores of the spinneret are in the shape of a gear; the number of teeth of the gear-shaped spinneret micropores of the spinneret is 7; the diameter of the gear-shaped spinneret micropores of the spinneret is 0.7 mm, and the gear-shaped tooth height is 0.17 mm; Step 8: After the spun silk fibers are oiled, they are curled on a winding machine at a temperature of 26° C. and a relative humidity of 55% to obtain polyester filaments.