Composite fiber material and preparation method thereof, electrode and display device

By using composite fiber material as an anode in quantum dot light emitting diodes, the problem of metal indium diffusion caused by ITO electrodes is solved, the stability and light output efficiency of the display device are improved, and the dependence on rare metals is reduced.

CN115679688BActive Publication Date: 2024-11-15GUANGDONG JUHUA PRINTING DISPLAY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111222858.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-20
Publication Date
2024-11-15
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

Traditional ITO electrodes cause metal indium diffusion due to heat treatment in quantum dot light-emitting diodes, resulting in poor stability of display devices, and the indium element is rare and has huge demand, making it difficult to meet application needs.

Method used

Composite fiber materials, including silver carbon fiber materials and silver nanowires, are prepared by heat treatment and hot pressing to form an internal uniform conductive path. The silver nanowires are embedded in the silver carbon fiber material to enhance conductivity and improve plasma coupling effect, and are used as display. The anode of the device.

Benefits of technology

The carrier transmission capability and the stability of the anode are improved, the light output efficiency and stability of the display device are enhanced, the stability problems caused by the diffusion of metal indium are avoided, and the use of silver nanowires reduces the dependence on rare metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115679688B_ABST
    Figure CN115679688B_ABST
Patent Text Reader

Abstract

The present invention relates to a composite fiber material and a preparation method thereof, an electrode and a display device. The composite fiber material comprises a silver carbon fiber material and silver nanowires, wherein the silver carbon fiber material comprises a carbon fiber material and silver particles distributed in the carbon fiber material, and the silver nanowires are embedded in the silver carbon fiber material. The composite fiber material can be used as an anode of a display device, which can improve the carrier transmission capacity and increase the stability of the anode, thereby improving the light extraction efficiency and stability of the display device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of display technology, and in particular to a composite fiber material and a preparation method thereof, an electrode and a display device. Background Art

[0002] With the rapid development of display technology, display devices such as quantum dot light-emitting diodes (QLEDs) have received widespread attention. Among them, quantum dot light-emitting diodes with semiconductor quantum dot materials as the light-emitting layer have broad application prospects in the fields of flat panel displays and solid-state lighting due to their good characteristics such as high color purity, high luminous efficiency, adjustable luminous color and device stability.

[0003] For quantum dot light-emitting diodes, the traditional anode is usually an ITO electrode. During the preparation of quantum dot light-emitting diodes, the ITO electrode will cause the appearance of metal indium (In) in the ITO film due to heat treatment. The diffusion of indium into the organic layer will generate a micro-area high electric field, thus forming dark spots in the quantum dot light-emitting layer, resulting in poor stability of the display device. Moreover, metal indium is a rare metal, with a content of about 0.1ppm in the earth's crust, and the demand for anodes is huge. Summary of the invention

[0004] Based on this, the present invention provides a composite fiber material and a preparation method thereof, an electrode and a display device, wherein the composite fiber material has good conductivity and stability.

[0005] The technical solution of the present invention to solve the above technical problems is as follows.

[0006] A composite fiber material comprises a silver carbon fiber material and silver nanowires, wherein the silver carbon fiber material comprises a carbon fiber material and silver particles distributed in the carbon fiber material, and the silver nanowires are embedded in the silver carbon fiber material.

[0007] In some embodiments, in the composite fiber material, the carbon fiber material is a carbon fiber material web, and the silver carbon fiber material is a silver carbon fiber film.

[0008] In some of the embodiments, in the composite fiber material, the ratio of the number of silver atoms in the silver particles to the number of carbon atoms in the carbon fiber material is (0.3-0.8):1.

[0009] In some embodiments, in the composite fiber material, the mass ratio of the silver nanowires to the silver particles is (0.4-2):1.

[0010] In some of the embodiments, in the composite fiber material, the aspect ratio of the carbon fibers in the carbon fiber material is (500-800):1.

[0011] In some embodiments, in the composite fiber material, the diameter of the silver nanowire is 20 nm to 30 nm, and the length is 10 μm to 20 μm.

[0012] The present invention provides a method for preparing the above-mentioned composite fiber material, comprising the following steps:

[0013] The silver salt, carbon fiber and organic solvent are mixed and then heat treated to obtain a silver carbon fiber material;

[0014] Silver nanowires are embedded in the silver carbon fiber material.

[0015] In some embodiments, in the method for preparing the composite fiber material, the silver salt is selected from at least one of silver nitrate, silver sulfate and silver chloride.

[0016] In some of the embodiments, in the method for preparing the composite fiber material, the carbon source is selected from at least one of polyacrylonitrile fiber, acetate fiber and polypropylene fiber.

[0017] In some of the embodiments, in the method for preparing the composite fiber material, the organic solvent is selected from at least one of DMF, DMAC and NMP.

[0018] In some embodiments, in the method for preparing the composite fiber material, the heat treatment is performed at 600° C. to 800° C. for 1 h to 5 h.

[0019] In some of the embodiments, in the method for preparing the composite fiber material, the silver nanowires are embedded in the silver carbon fiber material by using a hot pressing method.

[0020] The present invention provides an electrode, comprising the composite fiber material mentioned above.

[0021] The present invention provides a display device, comprising an anode, a light-emitting layer and a cathode which are stacked, wherein the anode comprises the composite fiber material.

[0022] In some of the embodiments, in the display device, the anode further comprises a metal reflective layer, and the metal reflective layer is disposed on a surface of the composite fiber material away from the light-emitting layer.

[0023] In some of the embodiments, in the display device, the display device further comprises a hole injection layer, and the hole injection layer is arranged between the anode and the light-emitting layer; the material of the hole injection layer is transition metal nitride.

[0024] In some of the embodiments, in the display device, the transition metal nitride is selected from at least one of tungsten nitride, nickel nitride, vanadium nitride and zirconium nitride.

[0025] In some of the embodiments, in the display device, the display device further comprises a hole transport layer, and the hole transport layer is arranged between the hole injection layer and the light-emitting layer; the material of the hole transport layer is a transition metal oxide.

[0026] In some of the embodiments, in the display device, the transition metal in the transition metal oxide is of the same type as the transition metal in the transition metal nitride.

[0027] Compared with the prior art, the composite fiber material of the present invention has the following beneficial effects:

[0028] The composite fiber material includes a silver carbon fiber material and silver nanowires, wherein the silver carbon fiber material includes a carbon fiber material and silver particles distributed in the carbon fiber material, so that the carbon fiber material and the silver particles form an internal uniform and continuous conductive path, effectively improving the conductivity of the composite fiber material; and the silver nanowires are embedded in the silver carbon fiber material, and the gap between the silver carbon fiber material and the silver nanowires has a strong plasma coupling effect, generating an electric field at the interface, further improving the conductivity of the composite fiber material. The composite fiber material can be used as an anode of a display device, which can improve the carrier transmission capacity, while also increasing the stability of the anode, thereby improving the light extraction efficiency and stability of the display device; avoiding the problem of poor stability of the display device caused by the diffusion of metal indium when using traditional ITO electrodes. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 is a schematic structural diagram of a composite fiber material in one embodiment;

[0031] Figure 2 A schematic diagram of a process flow of a composite fiber material in an anode in one embodiment;

[0032] Figure 3 Schematic diagram of the structure of a display device in one embodiment.

[0033] Description of reference numerals:

[0034] 10: composite fiber material; 11: silver carbon fiber material; 12: silver nanowire; 13: coating containing silver nanowire; 30: display device; 31: anode; 311: metal reflective layer; 32: light-emitting layer; 33: cathode; 34: substrate; 35: hole injection layer; 36: hole transport layer; 37: electron transport layer. DETAILED DESCRIPTION

[0035] The composite fiber material and preparation method thereof, electrode and display device of the present invention are further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0037] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0038] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0039] See also Figure 1 In one embodiment of the present invention, a composite fiber material 10 is provided. The composite fiber material 10 includes a silver carbon fiber material 11 and silver nanowires 12. The silver carbon fiber material 11 includes a carbon fiber material and silver particles distributed in the carbon fiber material. The silver nanowires 12 are embedded in the silver carbon fiber material 11.

[0040] In some examples, in the composite fiber material 10, the carbon fiber material is a carbon fiber material web, and the silver carbon fiber material 11 is a silver carbon fiber film. It can be understood that in this case, the composite fiber material 10 is a composite fiber film.

[0041] The above-mentioned composite fiber material distributes silver particles in the carbon fiber material, so that the carbon fiber material and the silver particles form an internal uniform and continuous conductive path, which effectively improves the conductivity of the composite fiber material; further, the silver nanowires are embedded in the silver carbon fiber material, and the gap between the silver carbon fiber material and the silver nanowires has a strong plasma coupling effect, which generates an electric field at the interface, further improving the conductivity of the composite fiber material; and the composite fiber material has good flexibility, which is conducive to the preparation of flexible devices.

[0042] In some of the examples, in the composite fiber material 10, the ratio of the number of silver atoms in the silver particles to the number of carbon atoms in the carbon fiber material is (0.3-0.8):1; optionally, the ratio of the number of silver atoms in the silver particles to the number of carbon atoms in the carbon fiber material is (0.3-0.5):1; preferably, the ratio of the number of silver atoms in the silver particles to the number of carbon atoms in the carbon fiber material is 0.5:1.

[0043] Controlling the ratio of the number of silver atoms in the silver particles to the number of carbon atoms in the carbon fiber material is beneficial to controlling the conductivity and light coupling ability of the anode material.

[0044] In some of the examples, in the composite fiber material 10, the mass ratio of silver nanowires to silver particles is (0.4-2):1; optionally, the mass ratio of silver nanowires to silver particles is (0.4-1.6):1; further, the mass ratio of silver nanowires to silver particles is (0.48-0.8):1; preferably, the mass ratio of silver nanowires to silver particles is 0.8:1.

[0045] In some of the examples, in the composite fiber material 10, the aspect ratio of the carbon fibers in the carbon fiber material is (500-800):1; optionally, the aspect ratio of the carbon fibers in the carbon fiber material is (500-600):1; preferably, the aspect ratio of the carbon fibers in the carbon fiber material is 500:1.

[0046] It can be understood that in some of the examples, when the carbon fiber material is a carbon fiber material mesh and the silver carbon fiber material is a silver carbon fiber film, the thickness of the carbon fiber mesh is 50nm to 100nm; optionally, the thickness of the carbon fiber mesh is 60nm to 80nm; preferably, the thickness of the carbon fiber mesh is 60nm.

[0047] In some of the examples, in the composite fiber material 10, the diameter of the silver nanowire is 20nm~50nm, and the length is 10μm~30μm; optionally, the diameter of the silver nanowire is 20nm~30nm, and the length is 10μm~20μm; preferably, the diameter of the silver nanowire is 25nm, and the length is 10μm.

[0048] See also Figure 2 An embodiment of the present invention provides a method for preparing the composite fiber material 10, comprising the following steps.

[0049] Step S110: mixing the silver salt, the carbon source and the first organic solvent and then performing heat treatment to obtain the silver carbon fiber film 11 .

[0050] In some of the examples, in step S110, the silver salt is selected from at least one of silver nitrate, silver sulfate and silver chloride; preferably, the silver salt is nitrate.

[0051] In some of the examples, in step S110, the carbon source is selected from at least one of polyacrylonitrile fiber, acetate fiber and polypropylene fiber; optionally, the carbon source is selected from at least one of polyacrylonitrile fiber and acetate fiber; preferably, the carbon source is polyacrylonitrile fiber.

[0052] In some of the examples, in step S110, the first organic solvent is selected from at least one of dimethylformamide (DMF), N,N-dimethylacetamide (DMAC) and methyl pyrrolidone (NMP); optionally, the first organic solvent is selected from at least one of dimethylformamide and N,N-dimethylacetamide; preferably, the first organic solvent is dimethylformamide.

[0053] In some specific examples, in step S110, a silver salt is added to a first organic solvent to dissolve, and then a carbon source is added and stirred to obtain a silver carbon fiber precursor solution, which is then heat treated.

[0054] In some of the examples, in step S110, the stirring temperature is 50°C to 80°C, and the stirring time is 1h to 5h; optionally, the stirring temperature is 50°C to 70°C, and the stirring time is 1h to 4h; preferably, the stirring temperature is 60°C, and the stirring time is 2h.

[0055] Furthermore, in some of the examples, before the step of heat treating the silver carbon fiber precursor solution in step S110, the method further includes the steps of sequentially performing a first electrospinning and removing the solvent on the silver carbon fiber precursor solution.

[0056] In some of the examples, in step S110, the voltage of the first electrospinning is 10 kV to 50 kV, and the time is 2 h to 5 h; optionally, the voltage of the first electrospinning is 10 kV to 30 kV, and the time is 2 h to 4 h; preferably, the voltage of the first electrospinning is 10 kV, and the time is 3 h.

[0057] In some of the examples, in step S110, the temperature used to remove the solvent is 100°C to 500°C; optionally, the temperature used to remove the solvent is 100°C to 350°C; preferably, the temperature used to remove the solvent is 280°C.

[0058] In some of the examples, in step S110, the heat treatment is performed at 600°C to 800°C for 1 hour to 5 hours; alternatively, the heat treatment is performed at 600°C to 700°C for 1 hour to 3 hours; preferably, the heat treatment is performed at 650°C for 1 hour.

[0059] In some examples, in step S110 , the heat treatment is performed under an argon atmosphere.

[0060] It can be understood that after the silver carbon fiber precursor solution containing silver salt and carbon source is heat-treated under the above-mentioned specific conditions, the silver salt and carbon source decompose to obtain a silver carbon fiber material, and the silver carbon fiber material is a silver carbon fiber film. Among them, the carbon source decomposes to form a carbon fiber mesh, and the silver salt is converted into silver particles distributed in the pores and surface of the carbon fiber mesh. It can be further understood that high-temperature heat treatment will increase the particle size of the silver particles, so the particle size of the silver particles distributed on the surface of the carbon fiber mesh is controlled by controlling the temperature and time of the heat treatment, and the silver particles distributed in the pores of the mesh carbon fiber are restricted by the pore size of the carbon fiber mesh, that is, the particle size of the silver particles in the pores of the mesh carbon fiber is the pore size of the mesh carbon fiber.

[0061] In some of the examples, in step S110, the particle size of the silver particles in the pores of the carbon fiber mesh is 30nm-50nm; optionally, the particle size of the silver particles in the pores of the carbon fiber mesh is 30nm-40nm.

[0062] In some of the examples, in step S110, the particle size of the silver particles on the surface of the carbon fiber mesh is 50nm-100nm; optionally, the particle size of the silver particles on the surface of the carbon fiber mesh is 50nm-80nm.

[0063] In some of the examples, in step S110, the thickness of the silver carbon fiber film is 50nm-150nm; optionally, the thickness of the silver carbon fiber film is 50nm-100nm; preferably, the thickness of the silver carbon fiber film is 100nm.

[0064] Step S120: embedding the silver nanowires 12 into the silver carbon fiber material 11 obtained in step S110.

[0065] In some of the examples, in step S120, the silver nanowires 12 are embedded in the silver carbon fiber material 11 by using a hot pressing method.

[0066] See also Figure 2 In some of the examples, in step S120, the silver nanowires 12 are mixed with a second organic solvent, coated on the silver carbon fiber material 11 obtained in step S110, the solvent is removed, and hot pressing is performed.

[0067] It can be understood that the silver nanowires 12 are mixed with the second organic solvent and then coated on the silver carbon fiber material 11 obtained in step S110 to form a thin coating 13 containing silver nanowires. After removing the solvent and hot pressing, the silver nanowires 12 are embedded in the silver carbon fiber material 11 to obtain a composite fiber material 10.

[0068] In some of the examples, in step S120, the second organic solvent is selected from at least one of ethanol, isopropanol and methanol; optionally, the second organic solvent is selected from at least one of ethanol and isopropanol; preferably, the second organic solvent is ethanol.

[0069] In some of the examples, in step S120, removing the solvent is performed by drying at 100° C. to 150° C. for 10 min to 30 min; in some of the specific examples, removing the solvent is performed by drying at 110° C. for 15 min.

[0070] In some of the examples, in step S120, the hot pressing is to apply a pressure of 10 MPa to 100 MPa for 3 min to 10 min at 30° C. to 100° C.; in some of the specific examples, a pressure of 30 MPa is applied at 50° C. for 5 min.

[0071] In some of the examples, in step S120 , thermal pressing is performed in a compressor.

[0072] An embodiment of the present invention provides an electrode, comprising any of the composite fiber materials 10 described above.

[0073] It is understood that the composite fiber material can be used directly as an electrode, or used together with other material layers as an electrode. In other words, the composite fiber material can be used directly as an anode or cathode, or used together with other material layers as an anode or cathode.

[0074] Another embodiment of the present invention provides an anode, comprising any of the composite fiber materials 10 described above.

[0075] In some of the examples, the composite fiber material 10 and the metal reflective layer are used together as an anode.

[0076] See also Figure 3In one embodiment of the present invention, a display device 30 is provided, comprising a stacked anode 31, a light-emitting layer 32 and a cathode 33. The anode 31 comprises the composite fiber material 10.

[0077] The anode of the display device contains the above-mentioned composite fiber material, which can improve the carrier transmission capacity and increase the stability of the anode, thereby improving the light output efficiency and stability of the display device, and avoiding the problem of poor stability of the display device caused by metal indium diffusion when using ITO electrodes.

[0078] In some of the embodiments, the anode 31 includes the composite fiber material 10 described above.

[0079] It can be understood that in some of the embodiments, the composite fiber material 10 is in the form of a film, and the anode 31 may further include a metal reflective layer 311 formed on the surface of the composite fiber film.

[0080] In some embodiments, in the anode 31 , the metal reflective layer 311 is disposed on a surface of the composite fiber material 10 away from the light emitting layer 32 .

[0081] Furthermore, the metal reflective layer 311 may be made of other metal materials such as silver.

[0082] It is understood that in some examples, the display device 30 further includes a substrate 34. Further, the anode 31, the light-emitting layer 32 and the cathode 33 are sequentially stacked on the substrate 34. It is also understood that when the anode 31 includes the metal reflective layer 311, the metal reflective layer 311, the composite fiber material 10, the light-emitting layer 32 and the cathode 33 are sequentially stacked on the substrate 34.

[0083] Further, the substrate 34 may be a rigid material or a flexible material.

[0084] In some of the examples, the display device 30 further includes a hole injection layer 35 , which is disposed between the anode 31 and the light-emitting layer 32 ; the hole injection layer 35 is made of transition metal nitride.

[0085] In some of the examples, in the display device 30, the transition metal nitride is selected from at least one of tungsten nitride (WN), nickel nitride (N2Ni3), vanadium nitride and zirconium nitride; optionally, the transition metal nitride is selected from at least one of tungsten nitride and nickel nitride; preferably, the transition metal nitride is tungsten nitride.

[0086] In some of the examples, in the display device 30 , the thickness of the hole injection layer 35 is 10 nm to 20 nm; optionally, the thickness of the hole injection layer 35 is 15 nm to 20 nm; preferably, the thickness of the hole injection layer 35 is 20 nm.

[0087] In some examples, the display device 30 further includes a hole transport layer 36 , which is disposed between the hole injection layer 35 and the light emitting layer 32 ; the hole transport layer 36 is made of a transition metal oxide.

[0088] In some of the examples, in the display device 30 , the transition metal oxide is selected from at least one of tungsten oxide, nickel oxide, vanadium oxide, and zirconium oxide.

[0089] It can be understood that the types of transition metals in transition metal oxides and transition metals in transition metal nitrides can be the same or different; preferably, the types of transition metals in transition metal oxides and transition metals in transition metal nitrides are the same. The hole injection layer 35 and the hole transport layer 36 use the same transition metal, so that there is no interface mismatch between the two thin films, which is more conducive to the transmission of holes and effectively improves the stability and light extraction efficiency of the display device.

[0090] It can also be understood that in some of the specific examples, in the display device 30, the transition metal nitride used as the material of the hole injection layer can be laser sintered to generate a transition metal oxide with the same metal element.

[0091] In some of the examples, in the display device 30 , the thickness of the hole transport layer 36 is 20 nm to 30 nm; optionally, the thickness of the hole transport layer 36 is 25 nm to 30 nm; preferably, the thickness of the hole transport layer 36 is 25 nm.

[0092] In some examples, the display device 30 further includes an electron transport layer 37 .

[0093] An embodiment of the present invention provides a method for manufacturing a display device 30 , including steps S100 to S700 .

[0094] Step S100 : forming an anode 31 on a substrate 34 .

[0095] It can be understood that the composite fiber material 10 is formed on the substrate 34 as the anode 31; or the metal reflective layer 311 is first formed on the substrate 34, and then the composite fiber material 10 is formed on the metal reflective layer 311, and the metal reflective layer 311 and the composite fiber material 10 together serve as the anode 31.

[0096] Step S200 : forming a hole injection layer 35 on the anode 31 .

[0097] In some of the examples, in step S200 , the hole injection layer 35 is prepared by an electrospinning method.

[0098] In some specific examples, step S200 includes steps S210 to S220.

[0099] Step S210: mixing an acid or salt containing a transition metal element, a binder and a third solvent to obtain a hole precursor solution;

[0100] Step S220: subjecting the hole precursor liquid to a second electrospinning process and then laser sintering in a nitrogen atmosphere.

[0101] It can be understood that the hole injection layer 35 includes a transition metal nitride fiber film.

[0102] It is also understood that in some of the examples, the transition element is selected from at least one of tungsten, nickel, vanadium and zirconium.

[0103] In some specific examples, in step S210, the acid or salt containing the transition metal element is selected from at least one of metatungstic acid, nickel nitrate, sodium vanadate and zirconium carbonate; further, the acid or salt containing the transition metal element is selected from at least one of metatungstic acid and nickel nitrate.

[0104] In some of the examples, in step S210, the binder is selected from at least one of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) and polyacrylamide (PAM); preferably, the binder is polyvinyl pyrrolidone.

[0105] In some of the examples, in step S210, the third solvent is selected from at least one of ethanol, water and isopropanol; preferably, the third solvent is a mixture of ethanol and water.

[0106] In some of the examples, in step S220, the voltage of the second electrospinning is 10 kV to 50 kV, and the time is 1 h to 2 h; optionally, the voltage of the second electrospinning is 10 kV to 30 kV, and the time is 1 h to 1.5 h; preferably, the voltage of the second electrospinning is 15 kV, and the time is 1 h.

[0107] In some of the examples, in step S220, the temperature of laser sintering is 600°C to 800°C; optionally, the temperature of laser sintering is 600°C to 700°C; preferably, the temperature of laser sintering is 600°C.

[0108] Step S300 : forming a hole transport layer 36 on the hole injection layer 35 .

[0109] In some examples, in step S300, the hole precursor solution prepared in step S210 is subjected to a third electrospinning process and then laser sintered in an oxygen atmosphere. It is understood that the hole transport layer includes a transition metal oxide fiber film.

[0110] In some of the examples, in step S300, the voltage of the third electrospinning is 10 kV to 50 kV, and the time is 2 h to 3 h; optionally, the voltage of the third electrospinning is 10 kV to 30 kV, and the time is 2 h to 2.5 h; preferably, the voltage of the third electrospinning is 15 kV, and the time is 2 h.

[0111] Step S400 : forming a light-emitting layer 32 on the hole transport layer 36 .

[0112] It is understandable that the light emitting layer 32 may be made of materials commonly used in the art, and the present invention does not limit this.

[0113] In some examples, in the display device 30, the light-emitting layer 32 is a quantum dot light-emitting layer 32, and the display device 30 is a quantum dot light-emitting diode 30. It is understood that the light-emitting layer 32 in the display device 30 can be a blue light-emitting layer, a red light-emitting layer, or a green light-emitting layer. It is understood that the type of the light-emitting layer 32 is not limited thereto, and in some examples, the light-emitting layer 32 can also be an organic light-emitting layer.

[0114] In some specific examples, in step S400 , the light emitting layer 32 is CdSe / ZnS, CdS / ZnSe or CdZnS / ZnSe.

[0115] In some of the examples, in step S400 , the thickness of the light emitting layer 32 is 30 nm to 60 nm; preferably, the thickness of the light emitting layer 32 is 30 nm.

[0116] Step S500 : forming an electron transport layer 37 on the light emitting layer 32 .

[0117] It is understandable that the electron transport layer 37 may be made of materials commonly used in the art, and the present invention does not limit this.

[0118] In some examples, in step S500 , the material of the electron transport layer 37 is zinc oxide, titanium oxide or Liq.

[0119] In some of the examples, in step S500 , the thickness of the electron transport layer 37 is 50 nm to 150 nm; preferably, the thickness of the electron transport layer 37 is 50 nm.

[0120] Step S600 : forming a cathode 33 on the electron transport layer 37 .

[0121] It is understandable that the cathode 33 may be made of materials commonly used in the art, and the present invention does not limit this.

[0122] In some examples, in step S400 , the cathode 33 is a silver electrode, an aluminum electrode or a copper electrode.

[0123] In some of the examples, in step S400 , the thickness of the cathode 33 is 20 nm to 100 nm; preferably, the thickness of the cathode 18 is 100 nm.

[0124] Step S700 : forming a packaging layer (not shown) on the cathode 33 to package the light-emitting layer 32 .

[0125] By using the composite fiber material provided above, the carbon fiber mesh film and the silver particles form a uniform and continuous conductive path inside, and the gap between the silver carbon fiber film and the silver nanowires has a strong plasma coupling effect and good conductivity; using the composite fiber material as the anode of the display device can improve the carrier transmission capacity, while also increasing the stability of the anode, thereby improving the light extraction efficiency and stability of the display device; further, using specific types of nitrides and oxides as the hole injection layer and the hole transport layer, respectively, increases the hole transport efficiency, improves the stability and conductivity of the film layer, thereby improving the light extraction efficiency and stability of the light-emitting device. Specific embodiments

[0127] The following examples are given according to the composite fiber material and the preparation method thereof, the electrode and the display device of the present invention. It should be understood that the composite fiber material and the preparation method thereof, the electrode and the display device of the present invention are not limited to the following examples.

[0128] Example 1

[0129] The specific structure of the display device provided in Example 1 is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (WN, 20nm) / hole transport layer (WO3, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0130] (1) Preparation of anode on substrate

[0131] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.48:1, add 0.22 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0132] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0133] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0134] 4) Dissolve 0.4 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0135] (2) Preparation of hole injection layer

[0136] Dissolve 10g of metatungstate in 10g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0137] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0138] (3) Preparation of hole transport layer

[0139] The hole precursor liquid prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the needle tip of the electrospinning container for 2 hours; then, laser sintering is performed at 600° C. for 1 hour in a nitrogen atmosphere to form a WO3 micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 25 nm.

[0140] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0141] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0142] (5) Preparation of encapsulation layer

[0143] Example 2

[0144] The specific structure of Example 2 is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / NiN (15nm) / NiO (25nm) / luminescent layer (CdSe / ZnS, 20nm) / zinc oxide (50nm) / silver (20nm) / encapsulation layer

[0145] (1) Preparation of anode on substrate

[0146] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.48:1, add 0.22 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0147] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0148] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0149] 4) Dissolve 0.4 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0150] (2) Preparation of hole injection layer

[0151] 8g of nickel nitrate was dissolved in 8g of ethanol aqueous solution, 12wt% PVP was added as a binder, and the mixture was stirred for 2h to obtain a hole precursor solution; the hole precursor solution was coated on the anode obtained in step (1), and a high voltage of 15kV was applied to the tip of the electrospinning container for 1h; then laser sintering was performed at 600℃ for 1h in a nitrogen atmosphere to form a tungsten nitride micro-nano fiber mesh film, which was the hole injection layer, with a film thickness of 20nm.

[0152] (3) Preparation of hole transport layer

[0153] The hole precursor solution prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 2 h; then, laser sintering is performed at 600 ° C for 1 h in a nitrogen atmosphere to form a NiO micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 25 nm.

[0154] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0155] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0156] (5) Preparation of encapsulation layer

[0157] Example 3

[0158] The specific structure of the display device provided in Example 3 is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (WN, 20nm) / hole transport layer (WO3, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0159] (1) Preparation of anode on substrate

[0160] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.5:1, add 0.18 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution to obtain a silver carbon fiber precursor solution.

[0161] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0162] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0163] 4) Dissolve 0.8 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0164] (2) Preparation of hole injection layer

[0165] Dissolve 10g of metatungstate in 10g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0166] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0167] (3) Preparation of hole transport layer

[0168] The hole precursor liquid prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the needle tip of the electrospinning container for 2 hours; then, laser sintering is performed at 600° C. for 1 hour in a nitrogen atmosphere to form a WO3 micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 25 nm.

[0169] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0170] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0171] (5) Preparation of encapsulation layer

[0172] Example 4

[0173] The specific structure of the display device provided in Example 4 is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (WN, 20nm) / hole transport layer (WO3, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0174] (1) Preparation of anode on substrate

[0175] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.8:1, add 0.11 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0176] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0177] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0178] 4) Dissolve 0.4 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0179] (2) Preparation of hole injection layer

[0180] Dissolve 10g of metatungstate in 10g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0181] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0182] (3) Preparation of hole transport layer

[0183] The hole precursor liquid prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the needle tip of the electrospinning container for 2 hours; then, laser sintering is performed at 600° C. for 1 hour in a nitrogen atmosphere to form a WO3 micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 25 nm.

[0184] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0185] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0186] (5) Preparation of encapsulation layer

[0187] Example 5

[0188] The specific structure of the display device provided in Example 5 is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (WN, 20nm) / hole transport layer (WO3, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0189] (1) Preparation of anode on substrate

[0190] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.48:1, add 0.22 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0191] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0192] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0193] 4) Dissolve 1.6 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0194] (2) Preparation of hole injection layer

[0195] Dissolve 10g of metatungstic acid in 810g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0196] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0197] (3) Preparation of hole transport layer

[0198] The hole precursor liquid prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the needle tip of the electrospinning container for 2 hours; then, laser sintering is performed at 600° C. for 1 hour in a nitrogen atmosphere to form a WO3 micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 25 nm.

[0199] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0200] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0201] (5) Prepare encapsulation layer.

[0202] Example 6

[0203] The specific structure of the display device provided in Example 6 is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (WN, 20nm) / hole injection layer (WO3, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0204] (1) Preparation of anode on substrate

[0205] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.48:1, add 0.22 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0206] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0207] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0208] 4) Dissolve 0.6 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0209] (2) Preparation of hole injection layer

[0210] Dissolve 10g of metatungstic acid in 810g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0211] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0212] (3) Preparation of hole transport layer

[0213] The hole precursor solution prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 2 h; then, laser sintering is performed at 600° C. for 1 h in a nitrogen atmosphere to form a WO3 micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 20 nm.

[0214] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0215] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0216] (5) Prepare encapsulation layer.

[0217] Example 7

[0218] The specific structure of the display device provided in the embodiment is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (WN, 20nm) / hole transport layer (NiO, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0219] (1) Preparation of anode on substrate

[0220] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.48:1, add 0.22 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0221] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0222] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0223] 4) Dissolve 0.4 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0224] (2) Preparation of hole injection layer

[0225] Dissolve 10g of metatungstate in 10g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0226] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0227] (3) Preparation of hole transport layer

[0228] 8g of nickel nitrate was dissolved in 8g of ethanol aqueous solution, 12wt% PVP was added as a binder, and the mixture was stirred for 2h to obtain a NiN precursor solution; the precursor solution was coated on the hole injection layer obtained in step (2), and a high voltage of 15kV was applied to the tip of the electrospinning container for 1h; then laser sintering was performed at 600℃ for 3h in a nitrogen atmosphere to form a nickel oxide micro-nano fiber mesh film, which was the hole transport layer, with a film thickness of 25nm.

[0229] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0230] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0231] (5) Preparation of encapsulation layer

[0232] Example 8

[0233] The specific structure of the display device provided in the embodiment is: substrate / Ag (150nm) / silver carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (PEDOT:PSS, 20nm) / hole transport layer (TFB, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0234] (1) Preparation of anode on substrate

[0235] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.48:1, add 0.22 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0236] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0237] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0238] 4) Dissolve 0.4 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0239] (2) Preparation of hole injection layer

[0240] The 20nm thick hole transport layer PEDOT:PSS was prepared by printing.

[0241] (3) Preparation of hole transport layer

[0242] TFB was prepared as a hole transport layer by printing method with a film thickness of 25 nm.

[0243] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0244] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0245] (5) Prepare encapsulation layer.

[0246] Comparative Example 1

[0247] ITO is used as the anode, ITO as the hole injection layer, PEDOT as the hole transport layer, and TFB as the quantum dot light-emitting layer; the specific structure is: substrate / Ag (140nm) / ITO (60nm) / PEDOT (20nm) / TFB (25nm) / RQD (20nm) / ZnO (30nm) / Ag (20nm).

[0248] Comparative Example 2

[0249] The specific structure of the display device provided in Comparative Example 2 is: substrate / Ag (150nm) / silver carbon fiber film (60nm) / hole injection layer (WN, 20nm) / hole transport layer (WO3, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0250] (1) Preparation of anode on substrate

[0251] 1) Dissolve 1 g of AgNO3 in 3 g of dimethylformamide (DMF), with the ratio of Ag atoms to C atoms being 0.48:1, add 0.22 g of polyacrylonitrile and stir at 60 °C for 2 h to form a light yellow solution, and obtain a silver carbon fiber precursor solution.

[0252] 2) placing the silver carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h to obtain a silver carbon fiber precursor.

[0253] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a silver carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0254] (2) Preparation of hole injection layer

[0255] Dissolve 10g of metatungstate in 10g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0256] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0257] (3) Preparation of hole transport layer

[0258] The hole precursor liquid prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the needle tip of the electrospinning container for 2 hours; then, laser sintering is performed at 600° C. for 1 hour in a nitrogen atmosphere to form a WO3 micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 25 nm.

[0259] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0260] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0261] (5) Preparation of encapsulation layer

[0262] Comparative Example 3

[0263] The specific structure of the display device provided in Comparative Example 3 is: substrate / Ag (150nm) / carbon fiber film embedded with silver nanowires (60nm) / hole injection layer (WN, 20nm) / hole transport layer (WO3, 25nm) / light-emitting layer (CdSe / ZnS, 20nm) / electron transport layer (zinc oxide, 50nm) / cathode (silver, 20nm) / encapsulation layer.

[0264] (1) Preparation of anode on substrate

[0265] 1) 0.22 g of polyacrylonitrile was dissolved in 3 g of dimethylformamide (DMF) and stirred at 60° C. for 2 h to form a light yellow solution to obtain a carbon fiber precursor solution.

[0266] 2) placing the carbon fiber precursor solution obtained in step 1) in an electrospinning container, applying a high voltage of 10 kV to the needle tip of the electrospinning container for 3 h, and obtaining a carbon fiber precursor.

[0267] 3) providing a substrate, forming a 150 nm silver layer on the substrate to obtain a substrate containing the silver layer; coating a carbon fiber precursor on the substrate containing the silver layer, removing the solvent at 280° C. in air, and then heat treating at 700° C. for 1 h in an Ar atmosphere to obtain a silver carbon fiber mesh film with an aspect ratio of 600:1; the film thickness is measured to be 60 nm.

[0268] 4) Dissolve 0.4 g of silver nanowires with a diameter of 25 nm and a length of 10 μm in 2 mL of ethanol solution, apply it on the silver carbon fiber mesh obtained in step 2), and bake it at 110° C. for 15 min to remove the solvent; then place it in a compressor and apply a pressure of 30 MPa for 5 min to obtain the product.

[0269] (2) Preparation of hole injection layer

[0270] Dissolve 10g of metatungstate in 10g of ethanol aqueous solution, add 12wt% PVP as a binder, and stir for 2h to obtain a cavity precursor solution;

[0271] The hole precursor liquid is coated on the anode prepared in step (1), and a high voltage of 15 kV is applied to the tip of the electrospinning container for 1 hour; then, laser sintering is performed at 600°C for 1 hour in a nitrogen atmosphere to form a tungsten nitride (WN) micro-nano fiber mesh film, which is the hole injection layer, with a film thickness of 20 nm.

[0272] (3) Preparation of hole transport layer

[0273] The hole precursor liquid prepared in step (2) is coated on the hole injection layer prepared in step (2), and a high voltage of 15 kV is applied to the needle tip of the electrospinning container for 2 hours; then, laser sintering is performed at 600° C. for 1 hour in a nitrogen atmosphere to form a WO3 micro-nano fiber mesh film, which is the hole transport layer, with a film thickness of 25 nm.

[0274] (4) Preparation of light-emitting layer, electron transport layer and cathode

[0275] A quantum dot light-emitting layer CdSe / ZnS 45nm, an electron transport layer zinc oxide film 50nm and a silver electrode 20nm are sequentially deposited on the hole transport layer prepared in step (3).

[0276] (5) Prepare encapsulation layer.

[0277] The ingredients or ratios of the embodiments and comparative examples are shown in Table 1.

[0278] Table 1

[0279]

[0280] The square resistance and transmittance of the anode in each embodiment and comparative example were tested. The square resistance of the anode film was tested using a four-probe instrument to characterize the conductivity of the thin film electrode. Generally, the larger the square resistance, the smaller the conductivity. The transmittance of the anode film was measured using a haze meter, and the ratio of transmitted light to incident light is the transmittance. The results are shown in Table 2.

[0281] The external quantum efficiency (EQE) and LT95@1000nit of the display devices prepared in various embodiments and comparative examples were tested, wherein LT95@1000nit refers to the time required for the brightness of 1000nit to decay to 950nit.

[0282] Table 2

[0283]

[0284] As can be seen from Table 2, as the mass ratio of silver atoms in the electrode increases, the conductivity of the thin film electrode becomes better, and the embedding of silver nanowires can further improve the conductivity of the thin film. At the same time, it can also couple light out through plasma resonance to increase the brightness of the device, thereby improving the device efficiency. While adopting this structure, while improving the conductivity and light transmittance of the electrode, the reduction of the potential barrier in the hole transport layer and the hole injection layer is more conducive to the transmission of carriers, thereby improving the device stability and thus increasing the device life.

[0285] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0286] The above-described embodiments only express several implementation methods of the present invention, which are convenient for understanding the technical solutions of the present invention in detail, but they cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided by the present invention are all within the protection scope of the claims attached to the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the contents of the attached claims, and the description and drawings can be used to interpret the contents of the claims.

Claims

1. A composite fiber material, characterized in that: It includes silver carbon fiber material and silver nanowires, wherein the silver carbon fiber material includes carbon fiber material and silver particles distributed in the carbon fiber material, the carbon fiber material is a carbon fiber material mesh, the silver carbon fiber material is a silver carbon fiber membrane, the silver particles are distributed in the pores and surface of the carbon fiber mesh; the silver nanowires are embedded in the silver carbon fiber material.

2. The composite fiber material according to claim 1, characterized in that The ratio of the number of silver atoms in the silver particles to the number of carbon atoms in the carbon fiber material is (0.3-0.8):

1.

3. The composite fiber material according to any one of claims 1 to 2, characterized in that: The mass ratio of the silver nanowires to the silver particles is (0.4-2):

1.

4. The composite fiber material according to any one of claims 1 to 2, characterized in that: The aspect ratio of the carbon fiber in the carbon fiber material is (500-800):

1.

5. The composite fiber material according to any one of claims 1 to 2, characterized in that: The diameter of the silver nanowire is 20nm-30nm, and the length is 10μm-20μm.

6. A method for preparing a composite fiber material, characterized in that: The following steps are involved: Mixing a silver salt, a carbon source and a first organic solvent, and sequentially subjecting the silver carbon fiber precursor solution obtained in the mixing step to a first electrostatic spinning and solvent removal treatment, and then to a heat treatment to obtain a silver carbon fiber material; The silver nanowires are mixed with a second organic solvent and coated on the silver carbon fiber material, the solvent is removed, and hot pressing is performed to embed the silver nanowires into the silver carbon fiber material.

7. The method for preparing a composite fiber material according to claim 6, characterized in that: The silver salt is selected from at least one of silver nitrate, silver sulfate and silver chloride; and / or The carbon source is selected from at least one of polyacrylonitrile fiber, acetate fiber and polypropylene fiber; and / or The first organic solvent is selected from at least one of DMF, DMAC and NMP; and / or The second organic solvent is selected from at least one of ethanol, isopropanol and methanol.

8. The method for preparing a composite fiber material according to claim 6, characterized in that: The heat treatment is performed at 600° C. to 800° C. for 1 h to 5 h.

9. The method for preparing a composite fiber material according to any one of claims 6 to 8, characterized in that: The silver nanowires are embedded in the silver carbon fiber material by using a hot pressing method.

10. An electrode, characterized in that: The composite fiber material comprises the composite fiber material according to any one of claims 1 to 5.

11. A display device, characterized in that: The invention comprises a stacked anode, a light-emitting layer and a cathode, wherein the anode comprises the composite fiber material according to any one of claims 1 to 5.

12. The display device according to claim 11, characterized in that The anode further comprises a metal reflective layer, and the metal reflective layer is arranged on a surface of the composite fiber material away from the light-emitting layer.

13. The display device according to claim 11 or 12, characterized in that: The display device further comprises a hole injection layer, which is arranged between the anode and the light-emitting layer; the material of the hole injection layer is transition metal nitride.

14. The display device according to claim 13, characterized in that The transition metal nitride is selected from at least one of tungsten nitride, nickel nitride, vanadium nitride and zirconium nitride.

15. The display device according to claim 14, characterized in that The display device further comprises a hole transport layer, wherein the hole transport layer is arranged between the hole injection layer and the light emitting layer; the material of the hole transport layer is a transition metal oxide.

16. The display device according to claim 15, characterized in that The transition metal in the transition metal oxide is of the same type as the transition metal in the transition metal nitride.