A Cu-based alloy solder, a silicon nitride ceramic copper-clad substrate using the solder, and a manufacturing method thereof
Through the brazing connection between Cu-based amorphous alloy brazing material and silicon nitride ceramic substrate, the problem of low copper clad bond strength of ceramic substrate is solved, and efficient and low-cost silicon nitride ceramic copper clad substrate is achieved.
Patent Information
- Application Number
- CN202110932744.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-08-13
AI Technical Summary
The existing ceramic substrate copper clad has problems such as low bonding strength, narrow process window, low production efficiency and high production costs.
Cu-based amorphous alloy brazing material is used, and the chemical composition is CuaTibZrcMdAleAgfSng. The thin strip of amorphous alloy is prepared by rapid solidification technology. It is used for the brazing connection between silicon nitride ceramic substrate and copper conductive layer, combining Zr, Ti, Hf, Elements such as Nb, Ta, Mo, Ni, Cr are added to improve binding force, and low-melting point alloys such as Al, Sn, and Ag are added to adjust the melting point.
It realizes high bonding strength between the ceramic substrate and the copper conductive layer, stabilizes the process window, improves production efficiency, reduces production costs, and is suitable for the packaging needs of high-power electronic devices.
Smart Images

Figure CN115703177B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic packaging, and specifically relates to a Cu-based alloy solder, a silicon nitride ceramic copper-clad substrate using the solder, and a manufacturing method thereof, and is particularly suitable for manufacturing a copper-clad ceramic substrate for high-power semiconductor devices. Background Art
[0002] Insulated gate bipolar transistor (IGBT) is the most important high-power device in the field of power electronics. It has outstanding advantages such as high operating frequency, high withstand voltage and large operating current. It is widely used in electric vehicles, photovoltaic grid-connected, wind power generation, electric locomotives, energy storage power stations, AC / DC conversion and frequency conversion control in high-voltage and high-current occasions in the industrial field. For high-power IGBT modules, in addition to chip technology, packaging technology is also very critical. Selecting appropriate packaging materials and processes and improving the heat dissipation capacity and reliability of the device are key issues that must be solved.
[0003] Ceramic substrates are widely used in high-power electronic device packaging due to their high insulation, high thermal conductivity, heat resistance, and low expansion. The heat generated by high-power electronic devices packaged with ceramic substrates can be dissipated through the high thermal conductivity ceramic copper-clad laminate to the shell. Since oxygen-free copper has a high thermal conductivity, the thermal conductivity of the ceramic copper-clad laminate is mainly determined by the thermal conductivity of the ceramic substrate material. At present, there are three main types of ceramics used as ceramic copper-clad laminate substrates, namely alumina ceramic substrates, aluminum nitride ceramic substrates, and silicon nitride ceramic substrates. Among them, silicon nitride (Si3N4) ceramics have the advantages of good thermal conductivity, high strength and fracture toughness, and excellent thermal fatigue resistance. It is a ceramic substrate material with good development prospects.
[0004] Copper cladding on ceramic substrate is a composite metal-ceramic substrate formed by directly bonding high-conductivity oxygen-free copper to the surface of a ceramic substrate at high temperature. It has the high thermal conductivity, high electrical insulation, high mechanical strength, low expansion and other characteristics of ceramics, as well as the high conductivity and excellent welding performance of oxygen-free copper. It is a key material for connecting chips and heat dissipation substrates in power module packaging in the field of power electronics.
[0005] There are three methods for copper coating on ceramic substrates. The first is the copper coating method on the ceramic surface. This method first attaches a metal transition layer to the ceramic substrate. The transition layer can be deposited on the surface of the ceramic substrate by vacuum sputtering. A metal seed layer, such as a Ti / Cu layer, can also be printed on the ceramic substrate by printing technology. Metal slurry, such as tungsten-molybdenum or molybdenum-manganese metallization slurry, is tightly bonded to the ceramic material after high-temperature sintering. Finally, copper is plated on the transition layer by electroplating / chemical plating to form a ceramic copper-clad substrate. The main disadvantage of this method is that the bonding strength between the electroplated copper layer and the ceramic substrate is low, which affects the reliability of the ceramic copper-clad board; in addition, the electroplating production speed is low, the thickness of the electroplated deposited copper layer is limited, it is difficult to meet the packaging requirements of high-current power devices, and the electroplating waste liquid is highly polluted. The second is the direct copper coating method for ceramics. This method is to heat at a high temperature of about 1063°C in oxygen-containing nitrogen, and directly weld a layer of copper foil on the surface of alumina or aluminum nitride ceramics. The basic principle is to use the copper-oxygen eutectic liquid phase formed by copper and oxygen at high temperature and low oxygen content to wet the two contacting material surfaces, namely the copper foil surface and the ceramic surface, and also react with alumina to achieve a strong bond between the copper foil and the ceramic. The disadvantages of this method are that the process is difficult, the yield is low, and it is only suitable for copper coating on the surface of aluminum oxide and aluminum nitride ceramics containing aluminum. The third is the active metal welding copper coating method, which uses a small amount of active elements contained in the solder, such as Ti and Zr, to react with ceramics to form a reaction layer that can be wetted by liquid solder, thereby achieving a method of bonding ceramics to metals. This method was originally used for welding alumina ceramics and metals. Commonly used solders include Ti-Ag-Cu and Zr-Ag-Cu, and then developed into active welding of aluminum nitride. The active metal welding substrate relies on the chemical reaction between ceramics and active metal solder paste at high temperature to achieve bonding, so its bonding strength is higher and the reliability is better. However, due to the high cost of this method, the small number of suitable solders, and the great influence of solder on the reliability of welding. Summary of the invention
[0006] The object of the present invention is to provide a Cu-based alloy solder, a silicon nitride ceramic copper-clad substrate using the solder and a manufacturing method thereof, so as to at least overcome one of the technical problems of the existing ceramic substrate copper-clad substrate having low bonding strength, narrow process window, low production efficiency and high production cost.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a Cu-based alloy solder, which is a Cu-based amorphous alloy, and the chemical composition is Cu a Ti b Zr c M d Al e Ag f Sn g, wherein M is one or more of Hf, Nb, Ta, Mo, Ni, and Cr, a, b, c, d, e, f, and g represent the atomic percentage of each element respectively, 40≤a≤65, 5≤b≤15, 5≤c≤15, 0≤d≤10, 1≤e≤15, 0≤f≤5, 10≤g≤30, and a+b+c+d+e+f+g=100.
[0009] Amorphous alloys are usually eutectic components with a low melting point, and the composition of amorphous alloys is not restricted by the phase diagram and can be adjusted arbitrarily. According to the common characteristics of amorphous alloys, the present invention combines the technical requirements of copper coating on silicon nitride ceramic substrates, and aims at the technical problems existing in the current copper coating on silicon nitride ceramics. A Cu-based amorphous alloy is proposed, and elements such as Zr, Ti, Hf, Nb, Ta, Mo, Ni, and Cr are added to the alloy, which is conducive to combining with silicon nitride ceramic substrates. At the same time, in order to lower the melting point of the alloy, low-melting-point alloys such as Al, Sn, and Ag are added to the alloy composition. In the technical solution proposed by the present invention, the alloy composition adopts all-metal elements, and does not contain metalloid elements and non-metallic elements. The reasons for the selection of the above components are as follows:
[0010] Cu is a matrix component of the solder. It is added for better wetting with the copper plate during the brazing process. If the content is too high, it is not conducive to the formation of an amorphous alloy ribbon because a large number of Cu nuclei are formed during the cooling process of the amorphous ribbon. If the content is too low, the melting point of the prepared amorphous ribbon as a solder is too high, even close to or higher than the melting point of Cu. In the solder provided by the present invention, the atomic percentage range of 40≤a≤65 is more suitable;
[0011] Ti is an active element, and is added to increase the bonding strength between the brazing filler metal and the ceramic substrate. The atomic percentage range of Ti is 5≤b≤15. If the atomic percentage exceeds 15, the melting point of the brazing filler metal increases rapidly, resulting in the melting point of the brazing filler metal being higher than that of Cu, and thus the brazing filler metal cannot be used. If the atomic percentage is less than 5, the bonding strength between the brazing filler metal and the silicon nitride ceramic substrate is low.
[0012] Zr is an amorphous forming element. It is added to increase the amorphous forming ability of the solder. The atomic percentage range of Zr is 5≤b≤15. If the atomic percentage exceeds 15, the melting point of the solder increases rapidly, resulting in the melting point of the solder being higher than that of Cu and being unusable. If the atomic percentage is less than 5, the amorphous forming ability of the solder is low, and it is difficult to prepare an amorphous alloy ribbon.
[0013] M, as an addible transition metal element, may be selected from at least one of Hf, Nb, Ta, Mo, Ni, and Cr, and is added to increase the amorphous forming ability of the solder;
[0014] Al is an active element and also an element for regulating the melting point of the solder. The atomic percentage range of Al is 1≤b≤15. If the atomic percentage exceeds 15, the melting point of the solder decreases rapidly, resulting in the need to lower the brazing temperature. The low brazing temperature affects the bonding strength between other active elements and the ceramic substrate. If the atomic percentage is less than 1, the bonding strength between the solder and the ceramic substrate is affected.
[0015] Ag is an active element, which is added to increase the bonding strength between the solder and the ceramic substrate. The atomic percentage range of Ag is 0≤b≤5. If the atomic percentage exceeds 5, the solder will be difficult to remove during the subsequent etching of the copper clad plate and the device package, which is not conducive to subsequent use. If this element is not added, the bonding strength between the solder and the ceramic substrate will be affected during the brazing process.
[0016] Sn is a low melting point element and is added to adjust the melting point of the solder. The appropriate atomic percentage range is 10≤b≤30. If the atomic percentage exceeds 30, it will affect the addition of other essential elements. If the atomic percentage is lower than 10, the melting point of the solder will be higher than that of Cu and cannot be used.
[0017] The chemical composition of the Cu-based alloy solder is composed of metal elements, and the sum of other impurity elements does not exceed 1 atomic percent.
[0018] The Cu-based alloy solder, as a preferred embodiment, has a+g≥65, 1≤d≤6, and f≤0.5. In this way, an amorphous strip with good plate shape can be prepared, and its surface quality and tolerance size can meet the needs of brazing. Cu and Sn are used as matrix materials, a+g≥65, which can ensure that the solder has a suitable melting point, the addition of M element in the range of 1≤d≤6 ensures that amorphous can be formed, and a small amount of Ag addition (f≤0.5) can ensure the activity of the solder and the silicon nitride substrate.
[0019] The above-mentioned Cu-based alloy solder, as a preferred embodiment, has a+g≥70, 1≤d≤6, 5≤e≤10, and f≤0.5. In this way, an amorphous strip with good plate shape can be prepared, and its surface quality and tolerance size can meet the needs of brazing. Cu and Sn are used as matrix materials, a+g≥70, which can ensure that the solder has a suitable melting point. The addition of M in the range of 1≤d≤6 ensures that amorphous can be formed. The addition of Al is limited to 5≤e≤10, which can better adjust the melting point of the solder and ensure the activity of the solder and the silicon nitride substrate. The addition of a small amount of Ag (f≤0.5) further enhances the activity of the silicon nitride substrate.
[0020] As a preferred embodiment, the Cu-based alloy solder is an amorphous alloy ribbon or an amorphous alloy powder.
[0021] The above-mentioned Cu-based alloy solder, as a preferred embodiment, is prepared by rapid solidification technology, and the prepared solder has a thin strip-type material with a thickness of 10-30μm (such as 12μm, 15μm, 20μm, 25μm, 28μm, etc.), and a more preferred thickness is 15-20μm (such as 15.5μm, 16μm, 17μm, 18μm, 19μm, 19.5μm, etc.).
[0022] The above-mentioned Cu-based alloy solder, as a preferred embodiment, is prepared by rapid solidification technology, and the width of the prepared solder is 10-200mm (for example, 20mm, 30mm, 50mm, 75mm, 100mm, 120mm, 150mm, 180mm, 190mm, etc.), and the more preferred width is 50-100mm (for example, 55mm, 60mm, 70mm, 80mm, 90mm, 95mm, etc.).
[0023] The Cu-based alloy solder is particularly suitable as a connecting layer material, which is placed between the silicon nitride ceramic substrate and the copper conductive layer to achieve a reliable connection between the silicon nitride ceramic substrate and the copper conductive layer through a brazing process.
[0024] In a second aspect, the present invention also provides a method for manufacturing the above-mentioned Cu-based alloy solder, which is prepared by rapid solidification technology, and can be prepared under vacuum conditions or under an argon protective atmosphere. Preferably, the raw materials are smelted by magnetic levitation smelting. If induction smelting is used, a calcium oxide crucible must be used.
[0025] The method for manufacturing the Cu-based alloy solder, as a preferred embodiment, comprises:
[0026] First, the raw materials are melted, and the highest temperature during the melting process is 1550-1750°C (such as 1560°C, 1580°C, 1600°C, 1650°C, 1680°C, 1700°C, 1720°C, 1740°C, etc.). After being fully alloyed, the temperature is lowered to 1120-1350°C (such as 1150°C, 1180°C, 1200°C, 1250°C, 1280°C, 1300°C, 1320°C, 1335°C, etc.), and cast into alloy rods;
[0027] Then, the alloy rod is remelted, and when the temperature of the molten alloy reaches 1120-1380°C (for example, 1130°C, 1150°C, 1180°C, 1200°C, 1250°C, 1300°C, 1330°C, 1350°C, etc.), the molten alloy is spray-cast onto a cooling roller with a linear speed of 18-35m / s (for example, 20m / s, 22m / s, 25m / s, 28m / s, 30m / s, 32m / s, 34m / s, etc.) at a pressure of 0.30-0.50MPa (for example, 0.32MPa, 0.35MPa, 0.40MPa, 0.45MPa, 0.48MPa, etc.) to obtain an alloy strip.
[0028] According to the alloy composition ratio proposed in the present invention, the strip is prepared by adopting the rapid solidification technology, that is, the molten alloy is poured through a nozzle onto a high-speed rotating cooling roller, and an amorphous alloy thin strip with a thickness of 10-30 microns, a width of about 200 mm, and a length of several thousand meters is prepared in one step, which has the advantages of simple production process and low material cost.
[0029] In a third aspect, the present invention also provides a silicon nitride ceramic copper-clad substrate, comprising a silicon nitride ceramic substrate, a copper foil, and a connecting layer located between the silicon nitride ceramic substrate and the copper foil and connecting the two, wherein the connecting layer is formed by brazing with the above-mentioned Cu-based alloy solder.
[0030] In the above-mentioned silicon nitride ceramic copper-clad substrate, generally speaking, the thickness of the connecting layer is slightly thinner than the thickness of the amorphous strip solder. At the connection between the connecting layer and the copper foil, components diffuse between the solder and the copper foil to form a diffusion layer; between the connecting layer and the silicon nitride ceramic substrate, active elements of the solder diffuse into the ceramic substrate; and the remaining solder forms an alloy after solidification.
[0031] In the above silicon nitride ceramic copper-clad substrate, as a preferred embodiment, the thickness of the silicon nitride ceramic substrate is 0.2-0.7 mm, and the thickness of the copper foil is 0.3-1.0 mm. Different semiconductor packaging devices have different requirements for the thickness of the silicon nitride ceramic substrate and the copper foil, which can be determined in practice according to the requirements of the packaging device.
[0032] In a fourth aspect, the present invention further provides a method for manufacturing the above-mentioned silicon nitride ceramic copper-clad substrate, comprising:
[0033] The silicon nitride ceramic substrate, the solder and the copper foil are stacked in this order;
[0034] The three stacked materials are placed in a fixture, and uniform pressure is applied on the stacked copper foil. The materials are then sent into a furnace for brazing, and then cooled in the furnace to obtain a silicon nitride copper-clad substrate.
[0035] The manufacturing method of the silicon nitride ceramic copper-clad substrate is a preferred embodiment, wherein the pressure treatment is to add 1.0*10 4 Pa-3.0*10 5 Pa (e.g. 5.0*10 4 Pa, 1.0*10 5 Pa, 1.5*10 5 Pa, 2.0*10 5 Pa, 2.5*10 5 Pa, 2.8*10 5 Pa, etc.) pressure.
[0036] The preparation method of the above-mentioned silicon nitride ceramic copper-clad substrate, as a preferred embodiment, the brazing treatment includes: heating at a heating rate of 10-50°C / min (such as 15°C / min, 20°C / min, 25°C / min, 30°C / min, 35°C / min, 40°C / min, 45°C / min, etc.), when the temperature reaches 1020-1060°C (such as 1025°C, 1030°C, 1035°C, 1040°C, 1045°C, 1050°C, 1055°C, etc.), keeping warm for 10-60min (such as 15min, 20min, 30min, 40min, 50min, 55min, etc.).
[0037] The amorphous alloy thin strip brazing material proposed in the present invention is used as a connecting layer material for the copper-clad silicon nitride ceramic substrate. When in use, the silicon nitride ceramic substrate, the connecting layer material and the copper foil are stacked in sequence, the three stacked materials are placed in a fixture, and uniform pressure is applied on the stacked copper foil, and then the whole is placed in a vacuum brazing furnace, heated to the liquidus temperature of the amorphous alloy thin strip for brazing. During the brazing process, one side of the connecting layer material is infiltrated and connected with the silicon nitride ceramic substrate, and the other side is infiltrated and connected with the copper foil. After cooling, a silicon nitride copper-clad substrate is formed. After brazing, the ceramic substrate and copper have a high bonding strength.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1) The Cu-based alloy brazing material proposed in the present invention has a melting point lower than and close to the melting point of copper, and is easy to perform vacuum brazing. At the same time, the alloy contains active metal elements that are easy to combine with the silicon nitride ceramic substrate, such as Zr, Ti, Nb, etc. After brazing, the bonding strength between the ceramic substrate and copper is high, and it is particularly suitable for the manufacture of silicon nitride ceramic copper-clad substrates;
[0040] 2) The Cu-based alloy brazing material proposed in the present invention has a stable preparation process. During use, brazing is performed at the liquidus temperature of the connecting layer material, and the process window is stable;
[0041] 3) The preparation and use method of the Cu-based alloy solder proposed in the present invention has a mature strip solder preparation process, a mature strip brazing process, and high production efficiency;
[0042] 4) The present invention proposes a connecting layer material for a silicon nitride ceramic copper-clad substrate, and a preparation and use method thereof. The production of the connecting layer material adopts a rapid solidification technology, and the production speed of the thin strip can reach 30m / s. When the thin strip is used, it is placed between the silicon nitride ceramic substrate and the copper, and after multi-layer stacking, it can be batch welded in a vacuum brazing furnace, and the production cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is the Cu proposed in Example 1 of the present invention. 60 Ti 10 Zr5Ni3Al 9.5 Ag 0.5 Sn 12 (at.%) XRD pattern of the alloy;
[0044] Figure 2 It is the Cu proposed in Example 2 of the present invention. 52 Ti8Zr7Nb2Al 12.5 Ag 0.5 Sn 18 (at.%) XRD pattern of the alloy. DETAILED DESCRIPTION
[0045] The present invention will be further described in detail below through embodiments in combination with the accompanying drawings. The protection scope of the present invention includes but is not limited to the following embodiments.
[0046] If no specific experimental steps or conditions are specified in the examples, the experiments can be carried out according to the conventional steps or conditions described in the literature in the art. All reagents and raw materials used in the examples are commercially available products.
[0047] Example 1
[0048] The brazing material for silicon nitride ceramic copper-clad substrate proposed in this embodiment and its preparation and use method are as follows: 60 Ti 10 Zr5Ni3Al 9.5 Ag 0.5 Sn 12(at.%) was prepared, with a total weight of 10 kg, and melted in a vacuum induction furnace. The highest temperature during the alloy melting process was 1720°C. After the alloy was fully alloyed, it was cooled to 1180°C and cast into an alloy rod with a diameter of 30 mm. The alloy rod was then loaded into a quartz tube of a vacuum spray belt and remelted with an induction coil. When the temperature of the alloy melt reached 1160°C, the alloy melt was sprayed on a copper cooling roller with a linear speed of 25 m / s using a pressure of 0.35 MPa to obtain an alloy thin strip with a thickness of 15-18 μm and a width of 20 mm. The XRD spectrum of the alloy is shown in the figure. Figure 1 As shown, it is shown that the alloy strip has an amorphous structure.
[0049] The amorphous alloy strip obtained in this example is used as solder, and the silicon nitride ceramic substrate, solder and copper foil are stacked in this order, wherein the thickness of the silicon nitride ceramic substrate is 0.5 mm, the thickness of the amorphous alloy strip is 15-18 μm, and the thickness of the copper foil is 0.3 mm. The stacked three materials are placed in a fixture, and 1.0*10 5 Pa pressure, and then put it into a vacuum brazing furnace as a whole, and heat it at a heating rate of 10℃ / min. When the temperature reaches 1050℃, keep it warm for 10min, then cool it to room temperature with the furnace, and take out the silicon nitride ceramic copper-clad substrate sample.
[0050] The peel strength between the silicon nitride ceramic substrate and the copper foil in the sample and the thermal cycling performance of the sample at -40℃-150℃ were measured. The brazed silicon nitride ceramic copper-clad substrate was cut into 10 identical samples and the peel strength between the silicon nitride ceramic substrate and the copper foil was measured. The measured value was 12-15N / mm 2 After 5000 hot and cold cycles, the peel strength between the silicon nitride ceramic substrate and the copper foil was measured to be 10-14N / mm. 2 .
[0051] Example 2
[0052] The present embodiment provides a connection layer material for a silicon nitride ceramic copper clad substrate and a preparation and use method thereof. 52 Ti8Zr7Nb2Al 12.5 Ag 0.5 Sn 18(at.%) was prepared, with a total weight of 10 kg, and melted in a vacuum induction furnace. The highest temperature during the alloy melting process was 1750°C. After sufficient alloying, the temperature was reduced to 1120°C and cast into an alloy rod with a diameter of 30 mm. The alloy rod was then loaded into a quartz tube of a vacuum spray belt and remelted with an induction coil. When the temperature of the alloy melt reached 1120°C, the alloy melt was sprayed on a copper cooling roller with a linear speed of 25 m / s at a pressure of 0.36 MPa to obtain an alloy thin strip with a thickness of 18-20 μm and a width of 20 mm. The XRD spectrum of the alloy is shown in FIG. Figure 2 As shown, it is shown that the alloy strip has an amorphous structure.
[0053] The amorphous alloy strip obtained in this example is used as solder, and the silicon nitride ceramic substrate, solder and copper foil are stacked in this order, wherein the thickness of the silicon nitride ceramic substrate is 0.64 mm, the thickness of the amorphous alloy strip is 18-20 μm, and the thickness of the copper foil is 0.5 mm. The stacked three materials are placed in a fixture, and 1.5*10 5 Pa pressure, and then put the whole into a vacuum brazing furnace, and heat it at a heating rate of 10℃ / min. When the temperature reaches 1030℃, keep it warm for 15min, and then cool it to room temperature with the furnace, and take out the silicon nitride ceramic copper-clad substrate sample.
[0054] The peel strength between the silicon nitride ceramic substrate and the copper foil in the sample and the thermal cycling performance of the sample at -40℃-150℃ were measured. The brazed silicon nitride ceramic copper-clad substrate was cut into 10 identical samples and the peel strength between the silicon nitride ceramic substrate and the copper foil was measured. The measured value was 10-14N / mm 2 After 5000 hot and cold cycles, the peel strength between the silicon nitride ceramic substrate and the copper foil was measured to be 9-12N / mm. 2 .
[0055] Finally, it should be noted that, if any, in the present invention, relational terms such as left and right, first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0056] Although the present disclosure has been disclosed above through the description of the specific embodiments of the present disclosure, it should be understood that those skilled in the art can design various modifications, improvements or equivalents to the present disclosure within the spirit and scope of the attached scheme. These modifications, improvements or equivalents should also be considered to be included in the scope of protection claimed by the present disclosure.
Claims
1. A Cu-based alloy solder, characterized in that: It is a Cu-based amorphous alloy with a chemical composition of Cu a Ti b Zr c M d Al e Ag f Sn g , wherein M is one or more of Hf, Nb, Ta, Mo, Ni, and Cr, a, b, c, d, e, f, and g respectively represent the atomic percentage of each element, 40≤a≤65, 5≤b≤15, 5≤c<15, 0≤d≤10, 1≤e≤15, 0≤f≤5, 10≤g≤30, a+b+c+d+e+f+g=100, and the solder is an amorphous alloy strip or an amorphous alloy powder.
2. The Cu-based alloy solder according to claim 1, characterized in that: a+g≥65, 1≤d≤6, f≤0.
5.
3. The Cu-based alloy brazing filler metal according to claim 1, characterized in that: a+g≥70, 1≤d≤6, 5≤e≤10, f≤0.
5.
4. The Cu-based alloy solder according to any one of claims 1 to 3, characterized in that: The solder is an amorphous alloy thin strip prepared by rapid solidification technology, with a thickness of 10-30 μm and a width of 10-200 mm.
5. The Cu-based alloy solder according to claim 4, characterized in that: The solder is an amorphous alloy thin strip prepared by rapid solidification technology, with a thickness of 15-20 μm and a width of 50-100 mm.
6. A method for manufacturing a Cu-based alloy solder as claimed in any one of claims 1 to 4, characterized in that: It is manufactured using rapid solidification technology under vacuum conditions or in an argon protective atmosphere.
7. The method for producing a Cu-based alloy solder according to claim 6, wherein: The raw materials are smelted by a magnetic suspension smelting method or an induction smelting method, and a calcium oxide crucible is used when the induction smelting is adopted.
8. The method for producing a Cu-based alloy solder according to claim 6, wherein: The manufacturing method of the Cu-based alloy solder comprises: First, the raw materials are melted, and the highest temperature during the melting process is 1550-1750℃. After being fully alloyed, the temperature is lowered to 1120-1350℃ and cast into alloy rods; Then the alloy rod is remelted, and when the temperature of the alloy melt reaches 1120-1380° C., the alloy melt is spray-casted on a cooling roller with a linear speed of 18-35 m / s at a pressure of 0.30-0.50 MPa to obtain an alloy strip.
9. A silicon nitride ceramic copper-clad substrate, characterized in that: The invention comprises a silicon nitride ceramic substrate, a copper foil and a connection layer located between the silicon nitride ceramic substrate and the copper foil and connecting the two. The connection layer is formed by brazing with the Cu-based alloy brazing material as claimed in any one of claims 1 to 5.
10. The silicon nitride ceramic copper-clad substrate according to claim 9, characterized in that: The thickness of the silicon nitride ceramic substrate is 0.2-0.7 mm, and the thickness of the copper foil is 0.3-1.0 mm.
11. A method for manufacturing a silicon nitride ceramic copper-clad substrate according to any one of claims 9 to 10, characterized in that: include: The silicon nitride ceramic substrate, the solder and the copper foil are stacked in this order; The three stacked materials are placed in a fixture, and uniform pressure is applied on the stacked copper foil. The materials are then sent into a furnace for brazing, and then cooled in the furnace to obtain a silicon nitride copper-clad substrate.
12. A method for manufacturing a silicon nitride ceramic copper-clad substrate as claimed in claim 11, characterized in that: include: The pressure treatment is to add 1.0×10 4 Pa -3.0×10 5 Pa pressure; The brazing process comprises: heating at a heating rate of 10-50° C. / min, and when the temperature reaches 1020-1060° C., keeping the temperature for 10-60 minutes.