A pure hydrocarbon condensed ring compound doped polymer long afterglow material and its preparation method and application
By physically doping pure hydrocarbon condensed ring aromatic compounds with melamine formaldehyde resin, the problem of unstable performance of polymer-based long afterglow materials at room temperature is solved, and efficient and stable long afterglow luminescence is achieved, which is suitable for a variety of practical purposes application.
Patent Information
- Application Number
- CN202211297892.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-10-21
AI Technical Summary
Existing polymer-based long afterglow materials are susceptible to water vapor and oxygen in the air at room temperature, and their performance is unstable, resulting in low luminescence efficiency and short life of the afterglow, making it difficult to achieve practical application.
The pure hydrocarbon condensed ring aromatic compound and melamine formaldehyde resin are used for physical doping. The crossover efficiency between exciton systems is improved through conjugation and rigid structure, which isolates oxygen and water vapor, and limits molecular movement, and prepares a polymerization with long afterglow luminescence properties. Materials.
Long afterglow luminescence is achieved at room temperature, with extended lifetime, high quantum yield and stable performance. It can maintain significant long afterglow luminescence in water, acid, alkali and organic solvents. It is suitable for anti-counterfeiting, data encryption and functional inks and other fields.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of luminescent materials, and in particular relates to a polymer long afterglow material doped with a pure hydrocarbon condensed ring compound, and a preparation method and application thereof. Background Art
[0002] The phenomenon of continuous luminescence after the excitation source stops excitation is usually called long afterglow luminescence. Due to the long afterglow luminescence property of the material, the influence of short-lived background light can be effectively eliminated, which can greatly improve the signal-to-noise ratio of the luminescence signal. Therefore, long afterglow materials have broad application prospects in the fields of intelligent transportation, emergency instructions, bioimaging, data encryption, and security and anti-counterfeiting. Ultra-long-lifetime (τ≥100ms) phosphorescence emission can cause long afterglow luminescence in organic matter. However, the triplet excitons that produce ultra-long-lifetime phosphorescence emission are easily quenched by temperature, water vapor and oxygen in the environment. In fact, most organic light-emitting materials can usually only produce afterglow emission at low temperatures (such as 77K) or inert atmospheres, and cannot truly achieve valuable practical applications.
[0003] In order to achieve organic long afterglow luminescence in ambient air atmosphere at room temperature, researchers have proposed many strategies, including: 1. Introducing heteroatoms and heavy halogen atoms into molecules to improve their intersystem crossing efficiency; 2. Providing a rigid environment for organic molecules through crystal engineering and forming special molecular aggregates; 3. Polymerizing organic molecules into polymers; 4. Incorporating organic molecules into solid matrices that can isolate oxygen and restrict molecular motion by host-guest doping; 5. Preparing carbon dots, etc. Among them, since the crystal material is rigid and the reproducibility of the phosphorescence performance of the material is not ideal, the introduction of heavy halogen atoms increases the phosphorescence intensity but shortens its phosphorescence lifetime. In contrast, polymers have a rich variety, high molecular weight and long chain structure, which can provide a rigid and dense matrix environment for phosphorescent molecules or chromophores, inhibit the thermal motion of molecules or groups in the system, and reduce contact with oxygen molecules in the air, which is conducive to the generation of long afterglow luminescence. In addition, polymers also have the advantages of rich variety, convenient processing, flexibility and low cost. Therefore, doping organic molecules into a polymer matrix or synthesizing polymers containing heteroatom chromophores has become an ideal strategy for obtaining organic long afterglow materials. Currently, the polymers commonly used to prepare organic long afterglow materials are mainly polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA), polylactic acid (PLA), polyacrylonitrile (PAN), etc. However, organic long afterglow materials prepared by host-guest doping with these polymers as the main body often have problems such as low afterglow luminescence efficiency, short life, and poor environmental resistance, which seriously limit their practical applications. In particular, their long afterglow luminescence performance is easily affected by water vapor and oxygen in the air at room temperature, and the performance decays significantly, the stability is poor, and even long afterglow luminescence cannot be produced within a few hours, and re-drying treatment is required. Therefore, the development of efficient and stable polymer long afterglow materials is of great practical significance. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the first aspect of the present invention provides a polymer long afterglow material, which exhibits a long afterglow phenomenon after being irradiated with light of 254nm, 290nm, 300nm, 350nm and 365nm wavelength at room temperature, and has excellent resistance to oxygen, water, alkali, acid and organic solvents.
[0005] The second aspect of the present invention provides a method for preparing the polymer long afterglow material.
[0006] The third aspect of the present invention provides a polymer long afterglow film comprising the polymer long afterglow material.
[0007] The fourth aspect of the present invention provides a method for preparing the polymer long afterglow film.
[0008] The fifth aspect of the present invention proposes an application of the polymer long afterglow material or the polymer long afterglow film.
[0009] According to a first aspect of the present invention, a polymer long afterglow material is provided, comprising a host component and a guest component doped in the host component, wherein the host component comprises melamine formaldehyde resin, and the guest component comprises a pure hydrocarbon condensed ring aromatic compound.
[0010] In the present invention, the planar pure hydrocarbon condensed ring aromatic compound molecules have high conjugation and strong rigidity. Therefore, in a dispersed state, the oscillator strength of its electronic transition is large, and the non-radiative transition efficiency of excitons is also low. At the same time, the melamine formaldehyde resin contains abundant nitrogen atoms and oxygen atoms, and has a covalently cross-linked three-dimensional network structure. This can not only enhance the spin-orbit coupling effect of the guest molecule, promote the intersystem crossing of its excited state electrons, but also effectively isolate oxygen and water vapor and limit molecular motion. The combined effect of these factors enables the prepared polymer material to produce an organic long afterglow with long life, high quantum yield and good performance stability.
[0011] In some embodiments of the present invention, the pure hydrocarbon fused ring aromatic compound comprises at least one of the compounds of formula (I) to formula (XI):
[0012]
[0013]
[0014] According to the different chemical structures of the doped guest molecules, the afterglow color, afterglow quantum yield, afterglow lifetime and other properties of the melamine formaldehyde resin-based long afterglow material can be regulated.
[0015] In some preferred embodiments of the present invention, the doping includes physical doping.
[0016] In some more preferred embodiments of the present invention, the mass fraction of the guest molecule is 0.001% to 5%, and more preferably 0.1% to 1%.
[0017] According to a second aspect of the present invention, a method for preparing a polymer long afterglow material is provided, comprising the following steps:
[0018] S1: adding melamine solid and formaldehyde aqueous solution to deionized water, adjusting the pH value of the solution with alkali, and heating to form a mixture solution;
[0019] S2: adding an organic solution of a pure hydrocarbon condensed ring aromatic compound to the mixed solution, heating for reaction, and then continuing to heat to evaporate the solvent to obtain the polymer long afterglow material.
[0020] In some embodiments of the present invention, the mass concentration of the formaldehyde aqueous solution is 1% to 55%, preferably 30% to 40%, and more preferably 37%.
[0021] In some preferred embodiments of the present invention, the molar ratio of melamine to formaldehyde is 1:(1-5), more preferably 1:(2-3).
[0022] In some more preferred embodiments of the present invention, the base includes any one of diethylamine, triethylamine, triethanolamine, sodium hydroxide, potassium hydroxide or sodium carbonate, and triethanolamine is further preferred.
[0023] In some more preferred embodiments of the present invention, the organic solvent of the organic solution includes any one of methanol, ethanol, acetone, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran or acetonitrile, and is more preferably tetrahydrofuran.
[0024] In some more preferred embodiments of the present invention, the pH value of the solution is 7.5-10, and more preferably 8-9.
[0025] In some more preferred embodiments of the present invention, in S1, the heating temperature is 60°C to 120°C, and more preferably 85°C to 95°C.
[0026] In some more preferred embodiments of the present invention, in S1, the heating time is 0.5h to 3h; more preferably 0.5h to 1h.
[0027] In some more preferred embodiments of the present invention, in S2, the temperature of the heating reaction is 60°C to 120°C, and more preferably 80°C to 100°C.
[0028] In some more preferred embodiments of the present invention, in S2, the heating reaction time is 1 h to 3 h.
[0029] In some more preferred embodiments of the present invention, in S2, the heating temperature is 120°C to 200°C, and more preferably 140°C to 160°C.
[0030] In some more preferred embodiments of the present invention, in S2, the heating time is 0.5h to 2h.
[0031] According to a third aspect of the present invention, a polymer long afterglow film is provided, comprising the polymer long afterglow material.
[0032] According to a fourth aspect of the present invention, a method for preparing the polymer long afterglow film is proposed, comprising the following steps: heating and pressing the polymer long afterglow material to obtain the polymer long afterglow film.
[0033] In some embodiments of the present invention, the heating and pressurizing time is 0.1 min to 15 min.
[0034] In some preferred embodiments of the present invention, the heating temperature is 130°C to 220°C, more preferably 150°C to 170°C.
[0035] In some more preferred embodiments of the present invention, the pressurized pressure is 1 MPa to 20 MPa, and more preferably 10 MPa.
[0036] According to a fifth aspect of the present invention, a use of the polymer long afterglow material or the polymer long afterglow film in data encryption and / or anti-counterfeiting and / or functional ink and / or road marking is proposed.
[0037] The beneficial effects of the present invention are:
[0038] 1. The present invention uses pure hydrocarbon condensed ring aromatic compounds as the guest and melamine formaldehyde resin as the main body, and can easily prepare a polymer long afterglow material through physical doping, and can adjust the long afterglow luminescence performance of the prepared material by changing the chemical structure of the guest molecule.
[0039] 2. The polymer long afterglow material of the present invention can effectively inhibit the penetration of solvent molecules at room temperature, and can still produce significant long afterglow luminescence even if immersed in water, dilute hydrochloric acid, alkali solution and organic solvent for more than 7 days, which can solve the problem that the long afterglow luminescence performance of current polymer-based long afterglow materials is unstable in air and in solvent atmosphere.
[0040] 3. The polymer long afterglow material of the present invention not only has the characteristics of long afterglow luminescence life, high efficiency and adjustable color, but also has good performance stability. Therefore, the material has strong practicality in the fields of anti-counterfeiting, data encryption, functional ink, road marking, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:
[0042] Figure 1 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (I) in Example 1 of the present invention is shown in FIG.
[0043] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of the compound of formula (II) in Example 2 of the present invention.
[0044] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of the compound of formula (III) in Example 3 of the present invention.
[0045] Figure 4 This is the hydrogen nuclear magnetic resonance spectrum of the compound of formula (IV) in Example 4 of the present invention.
[0046] Figure 5 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (V) in Example 5 of the present invention is shown in FIG.
[0047] Figure 6 This is the hydrogen nuclear magnetic resonance spectrum of the compound of formula (VI) in Example 6 of the present invention.
[0048] Figure 7 This is a process diagram of preparing the polymer long afterglow material into a translucent sheet by a hot pressing method in Example 7 of the present invention.
[0049] Figure 8 This is a diagram showing the application of the polymer long afterglow material prepared in Example 2 and Example 4 in Example 8 of the present invention in anti-counterfeiting and information encryption.
[0050] Fig. 9 These are pictures of the solid powders (microcrystals) of the compounds of formula (I) to (VI) in Examples 1 to 6 of the present invention under ultraviolet light and after the ultraviolet light is turned off.
[0051] Fig.10 This is a steady-state luminescence spectrum diagram of the solid powder (microcrystals) of the compound of formula (I) to the compound of formula (VI) in Examples 1 to 6 of the present invention.
[0052] Fig.11 The luminescence decay curves of the solid powders (microcrystals) of the compounds of formula (I) to (VI) in Examples 1 to 6 of the present invention and the lifetime values obtained by fitting are shown.
[0053] Fig.12 These are steady-state luminescence spectra and afterglow luminescence spectra of the polymer long afterglow materials prepared in Examples 1 to 6 of the present invention.
[0054] Fig.13 The luminescence attenuation curves of the polymer long afterglow materials prepared in Examples 1 to 6 of the present invention and the afterglow luminescence lifetime values obtained by fitting are shown.
[0055] Fig.14 This is a diagram of the afterglow luminescence phenomenon of the polymer long afterglow material prepared in Examples 1 to 6 of the present invention at room temperature.
[0056] Fig.15 The afterglow luminescence spectra of the polymer long afterglow material prepared in Example 6 of the present invention at different temperatures.
[0057] Fig.16 The CIE chromaticity coordinate diagram of the afterglow luminescence color of the polymer long afterglow material prepared in Example 6 of the present invention at different temperatures.
[0058] Fig.17 These are long afterglow luminescence images of the polymer long afterglow material prepared in Example 1 of the present invention after being immersed in different organic solvents for 7 days.
[0059] Fig.18 These are pictures of the polymer film materials prepared in Comparative Examples 1 to 4 of the present invention under irradiation with ultraviolet light and after the ultraviolet light is turned off. DETAILED DESCRIPTION
[0060] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0061] The nuclear magnetic resonance hydrogen spectra of the compounds of formula (I) to formula (VI) in the following examples correspond to the following: Figures 1 to 6 shown.
[0062] Example 1
[0063] This embodiment prepares a polymer long afterglow material, which is a melamine formaldehyde resin-based long afterglow material I@MF doped with a compound of formula (I). The specific process is as follows:
[0064] S1: Weigh 6 mg of the compound of formula (I) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (I) with a concentration of 3 mg / mL;
[0065] S2: 6.3 g of melamine and 10.1 mL of a 37% formaldehyde aqueous solution were added into a reaction vessel, and triethanolamine was added to adjust the pH value of the solution to 8-9, and the solution was heated at 90° C. for 1 h to form a clear mixed solution.
[0066] S3: Take 2 mL of the organic solution of the compound of formula (I) in S1 and add it to 1 mL of the mixed solution prepared by S2, shake it quickly and evenly, then heat it at 85°C for 2 hours, then increase the temperature to 160°C and continue heating for 1 hour. After the solvent is evaporated, the melamine formaldehyde resin-based long afterglow material Ⅰ@MF doped with formula (I) is obtained.
[0067] Example 2
[0068] This embodiment prepares a polymer long afterglow material, which is a melamine formaldehyde resin-based long afterglow material II@MF doped with a compound of formula (II). The specific process is as follows:
[0069] S1: Weigh 1 mg of the compound of formula (II) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (II) with a concentration of 1 mg / mL;
[0070] S2: 6.3 g of melamine and 10.1 mL of a 37% formaldehyde aqueous solution were added into a reaction vessel, and triethanolamine was added to adjust the pH value of the solution to 8-9, and the solution was heated at 90° C. for 1 h to form a clear mixed solution.
[0071] S3: Take 1 mL of the organic solution of the compound of formula (II) in S1 and add it to the mixed solution prepared by 1.5 mL of S2, shake it quickly and evenly, then heat it at 100°C for 2 hours, then increase the temperature to 160°C and continue heating for 0.5 hours. After the solvent is evaporated, the melamine formaldehyde resin-based long afterglow material II@MF doped with formula (II) is obtained.
[0072] Example 3
[0073] This embodiment prepares a polymer long afterglow material, which is a melamine formaldehyde resin-based long afterglow material III@MF doped with a compound of formula (III). The specific process is as follows:
[0074] S1: Weigh 1 mg of the compound of formula (III) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (III) with a concentration of 1 mg / mL;
[0075] S2: 6.3 g of melamine and 10.1 mL of a 37% formaldehyde aqueous solution were added into a reaction vessel, and triethanolamine was added to adjust the pH value of the solution to 8-9, and the solution was heated at 90° C. for 1 h to form a clear mixed solution.
[0076] S3: Take 1 mL of the organic solution of the compound of formula (III) in S1 and add it to 1.5 mL of the mixed solution prepared in S2, shake it quickly and evenly, then heat it at 100°C for 2 hours, then increase the temperature to 150°C and continue heating for 1 hour. After the solvent is evaporated, the melamine formaldehyde resin-based long afterglow material III@MF doped with formula (III) is obtained.
[0077] Example 4
[0078] This embodiment prepares a polymer long afterglow material, which is a melamine formaldehyde resin-based long afterglow material IV@MF doped with a compound of formula (IV). The specific process is as follows:
[0079] S1: Weigh 1 mg of the compound of formula (IV) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (IV) with a concentration of 1 mg / mL;
[0080] S2: 6.3 g of melamine and 10.1 mL of a 37% formaldehyde aqueous solution were added into a reaction vessel, and triethanolamine was added to adjust the pH value of the solution to 8-9, and the solution was heated at 90° C. for 1 h to form a clear mixed solution.
[0081] S3: Take 1 mL of the organic solution of the compound of formula (IV) in S1 and add it to 1.5 mL of the mixed solution prepared by S2, shake it quickly and evenly, then heat it at 85°C for 2 hours, then increase the temperature to 160°C and continue heating for 0.5 hours. After the solvent is evaporated, the melamine formaldehyde resin-based long afterglow material IV@MF doped with formula (IV) is obtained.
[0082] Example 5
[0083] This embodiment prepares a polymer long afterglow material, which is a melamine formaldehyde resin-based long afterglow material V@MF doped with a compound of formula (V). The specific process is as follows:
[0084] S1: Weigh 5 mg of the compound of formula (V) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (V) with a concentration of 2.5 mg / mL;
[0085] S2: 6.3 g of melamine and 10.1 mL of a 37% formaldehyde aqueous solution were added into a reaction vessel, and triethanolamine was added to adjust the pH value of the solution to 8-9, and the solution was heated at 90° C. for 1 h to form a clear mixed solution.
[0086] S3: Take 2.5 mL of the organic solution of the compound of formula (V) in S1 and add it to 1.5 mL of the mixed solution prepared by S2, and shake it quickly and evenly, then heat it at 100°C for 2 hours, then increase the temperature to 160°C and continue heating for 1 hour. After the solvent is evaporated, the melamine formaldehyde resin-based long afterglow material V@MF doped with formula (V) is obtained.
[0087] Example 6
[0088] This embodiment prepares a polymer long afterglow material, specifically a melamine formaldehyde resin-based long afterglow material VI@MF doped with a compound of formula (VI). This embodiment includes the following three steps:
[0089] S1: Weigh 2 mg of the compound of formula (VI) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (VI) with a concentration of 0.1 / mL;
[0090] S2: 6.3 g of melamine and 10.1 mL of a 37% formaldehyde aqueous solution were added into a reaction vessel, and triethanolamine was added to adjust the pH value of the solution to 8-9, and the solution was heated at 90° C. for 1 h to form a clear mixed solution.
[0091] S3: Take 2 mL of the organic solution of the compound of formula (VI) in S1 and add it to 7 mL of the mixed solution prepared by S2, shake it quickly and evenly, then heat it at 105°C for 1 hour, then increase the temperature to 160°C and continue heating for 0.5 hour. After the solvent is evaporated, the melamine formaldehyde resin-based long afterglow material VI@MF doped with formula (VI) is obtained.
[0092] Example 7
[0093] This example prepares a polymer long afterglow film, and the specific process is as follows:
[0094] The polymer long afterglow material prepared in Example 1 was heated and pressurized at 150° C. and 10 MPa for 5 minutes using a hot press to prepare a translucent plastic sheet.
[0095] The polymer long afterglow material prepared in Example 2 was heated and pressurized at 150° C. and 10 MPa for 5 minutes using a hot press to prepare a translucent plastic sheet.
[0096] The polymer long afterglow material prepared in Example 3 was heated and pressurized at 160° C. and 10 MPa for 5 minutes using a hot press to prepare a translucent plastic sheet.
[0097] The polymer long afterglow material prepared in Example 4 was heated and pressurized at 150° C. and 10 MPa for 10 min using a hot press to prepare a translucent plastic sheet.
[0098] The polymer long afterglow material prepared in Example 5 was heated and pressurized at 160° C. and 10 MPa for 5 minutes using a hot press to prepare a translucent plastic sheet.
[0099] The polymer long afterglow material prepared in Example 6 was heated and pressurized at 160° C. and 10 MPa for 10 min using a hot press to prepare a translucent plastic sheet.
[0100] In Examples 1 to 6, the polymer long afterglow material is prepared into a translucent sheet by hot pressing. Figure 7 shown.
[0101] Example 8
[0102] In this embodiment, a melamine formaldehyde resin-based long afterglow material doped with a compound of formula (II) and a melamine formaldehyde resin-based long afterglow material doped with a compound of formula (IV) are prepared into a composite two-dimensional code for anti-counterfeiting and information encryption. The specific steps are as follows:
[0103] S1: Weigh 1 mg of the compound of formula (IV) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (IV) with a concentration of 1 mg / mL;
[0104] S2: 6.3 g of melamine and 10.1 mL of a 37% formaldehyde aqueous solution were added into a reaction vessel, and triethanolamine was added to adjust the pH value of the solution to 8-9, and the solution was heated at 90° C. for 1 h to form a clear mixed solution.
[0105] S3: Take 1 mL of the organic solution of the compound of formula (IV) in S1 and add it to 1.5 mL of the mixed solution prepared in S2, shake it quickly and evenly, and then use it as ink to print a QR code with the identifiable information "South China Normal University" on paper using screen printing technology;
[0106] S4: The two-dimensional code pattern in S3 was heated at 100° C. for 2 h, and then the temperature was raised to 160° C. and heated for 1 h to prepare a heat-cured IV@MF-based two-dimensional code.
[0107] S5: Weigh 1 mg of the compound of formula (II) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (II) with a concentration of 1 mg / mL;
[0108] S6: Take 1 mL of the organic solution of the compound of formula (II) in S5 and add it to the mixed solution prepared by 1.5 mL of S2, and shake it quickly to make it uniform. Then, use it as ink to print a QR code that can identify the information "Explore Science and Nature" at the same position of the QR code in S4;
[0109] S7: The two-dimensional code pattern in S6 was heated at 100° C. for 2 h, and then heated to 160° C. for further 1 h to prepare a heat-cured II@MF-based two-dimensional code. The two overlapping two-dimensional codes formed a composite two-dimensional code pattern.
[0110] The prepared composite pattern cannot read the correct information through QR code scanning under sunlight. The blue and yellow QR codes presented by the long afterglow produced by 254nm and 365nm ultraviolet light irradiation need to be scanned respectively to read the corresponding information, thereby playing the role of anti-counterfeiting and information encryption. The results are as follows Figure 8 shown.
[0111] from Figure 8 It can be seen that the polymer long afterglow material prepared by the present invention can be applied to the fields of anti-counterfeiting, information encryption, functional ink, etc.
[0112] Comparative Example 1
[0113] This comparative example prepares a polymer film material doped with polymethyl methacrylate by a molecule of formula (I). The difference from Example 1 is that the doped polymer is replaced with polymethyl methacrylate. The specific process is as follows:
[0114] S1: Weigh 10 mg of the compound of formula (I) and 1000 mg of polymethyl methacrylate, add them into 5 mL of dichloromethane, and let stand for 1 hour to form a clear mixed solution;
[0115] S2: Put the mixed solution in S1 into a mold, let it stand for 12 hours to evaporate the solvent, heat it at 100° C. for 3 hours, and demold to obtain a polymer film material (I)@PMMA doped with polymethyl methacrylate of formula (I).
[0116] Comparative Example 2
[0117] This comparative example prepares a polymer film material doped with polyvinyl alcohol by a molecule of formula (I). The difference from Example 1 is that the doped polymer is replaced with polyvinyl alcohol. The specific process is as follows:
[0118] S1: Weigh 3 mg of the compound of formula (I) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (I) with a concentration of 1 mg / mL;
[0119] S2: 5.0 g of polyvinyl alcohol was added to deionized water and heated at 100 °C for 12 h to form a clear polyvinyl alcohol solution with a concentration of 50 mg / mL;
[0120] S3: Take 1 mL of the organic solution of the compound of formula (I) in S1 and add it to 2 mL of the polyvinyl alcohol solution prepared in S2, shake it rapidly and ultrasonicate it to make it uniform. Put the mixed solution into a mold, heat it at 80°C for 6 hours, and then demold it to obtain a polymer film material (I)@PVA doped with polymethyl methacrylate of formula (I).
[0121] Comparative Example 3
[0122] This comparative example prepares a polymer film material doped with polymethyl methacrylate by a molecule of formula (IV). The difference from Example 4 is that the doped polymer is replaced with polymethyl methacrylate. The specific process is as follows:
[0123] S1: Weigh 1 mg of the compound of formula (IV) and 1000 mg of polymethyl methacrylate, add them into 5 mL of dichloromethane, and let stand for 1 hour to form a clear mixed solution;
[0124] S2: Place the mixed solution in S1 into a mold, allow to stand for 12 hours to evaporate the solvent, heat at 100° C. for 3 hours, and demold to obtain a polymer film material (IV)@PMMA doped with polymethyl methacrylate of formula (IV).
[0125] Comparative Example 4
[0126] This comparative example prepares a polymer film material doped with polyvinyl alcohol by a molecule of formula (IV). The difference from Example 4 is that the doped polymer is replaced with polyvinyl alcohol. The specific process is as follows:
[0127] S1: Weigh 3 mg of the compound of formula (I) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (I) with a concentration of 1 mg / mL;
[0128] S2: 5.0 g of polyvinyl alcohol was added to deionized water and heated at 100 °C for 12 h to form a clear polyvinyl alcohol solution with a concentration of 50 mg / mL;
[0129] S3: Take 0.1 mL of the organic solution of the compound of formula (I) in S1 and add it to 2 mL of the polyvinyl alcohol solution prepared in S2, shake it rapidly and ultrasonicate it to make it uniform. Put the mixed solution into a mold, heat it at 80°C for 6 hours, and then demold it to obtain a polymer film material (IV)@PVA doped with polyvinyl alcohol of formula (IV).
[0130] Test example
[0131] This test example tests the optical properties of the solid powders (microcrystals) of the compounds of formula (I) to (VI) in Examples 1 to 6, the polymer long afterglow materials in Examples 1 to 6, and the polymer film materials in Comparative Examples 1 to 4. The main properties of the target materials, such as the afterglow luminescence spectrum, afterglow quantum yield, afterglow lifetime, and the stability of the afterglow performance, are investigated. All tests were conducted on an Edinburgh FLS980 steady-state transient fluorescence spectrometer with an integrating sphere. The results are shown in the figure. Figures 9 to 18 , as shown in Table 1.
[0132] Fig. 9 These are pictures of the solid powders (microcrystals) of the compounds of formula (I) to (VI) in Examples 1 to 6 under ultraviolet light and after the ultraviolet light is turned off.
[0133] Fig.10 It is the steady-state luminescence spectra of the solid powders (microcrystals) of the compounds of formula (I) to (VI) in Examples 1 to 6.
[0134] Fig.11 The luminescence decay curves of the solid powders (microcrystals) of the compounds of formula (I) to (VI) in Examples 1 to 6 and the lifetime values obtained by fitting are shown.
[0135] Fig.12 The steady-state luminescence spectra and afterglow luminescence spectra of the polymer long afterglow materials prepared in Examples 1 to 6 are shown.
[0136] Fig.13 The luminescence attenuation curves of the polymer long afterglow materials prepared in Examples 1 to 6 and the afterglow luminescence lifetime values obtained by fitting are shown.
[0137] Fig.14This is a diagram of the afterglow luminescence phenomenon of the polymer long afterglow material prepared in Examples 1 to 6 at room temperature.
[0138] Fig.15 The afterglow luminescence spectra of the polymer long afterglow material prepared in Example 6 at different temperatures.
[0139] Fig.16 The CIE chromaticity coordinate diagram of the afterglow luminescence color of the polymer long afterglow material prepared in Example 6 at different temperatures.
[0140] Fig.17 The polymer long afterglow material prepared in Example 1 was mixed with water and sodium hydroxide aqueous solution (10 -2 M), hydrochloric acid (10 -2 M), acetic acid, acetone, acetonitrile, dichloromethane, N,N-dimethylformamide, ethyl acetate, ethanol, n-hexane, tetrahydrofuran, toluene and other common organic solvents after immersion for 7 days.
[0141] Fig.18 These are pictures of the polymer film materials prepared in Comparative Examples 1 to 4 of the present invention under irradiation with ultraviolet light and after the ultraviolet light is turned off.
[0142] Table 1 Test results of photophysical properties of polymer long afterglow materials in Examples 1 to 6
[0143]
[0144] from Figures 9 to 11 It can be seen that at room temperature, the pure compounds of formula (I) to (VI) did not produce obvious long afterglow luminescence after being excited by ultraviolet light. Pure guest materials only emit instantaneous fluorescence in the solid state and have no afterglow properties. They need to be doped into the host material to produce long afterglow luminescence.
[0145] From Table 1, Figure 7 and Figure 12 to Figure 14 It can be seen that the polymer long afterglow materials prepared in Examples 1 to 6 all have long afterglow luminescence characteristics, and their afterglow lifetime can reach up to 4.5s at room temperature in air, and their highest efficiency can reach 22.67%. At the same time, their long afterglow luminescence wavelength, lifetime and efficiency can be adjusted by changing the doped guest molecules.
[0146] from Figure 15-16 It can be seen that the polymer long afterglow material prepared in Example 6 can also change the color of the afterglow by regulating the temperature. (VI) @MF material changes the color of the afterglow from yellow-green to white to blue as the temperature increases in the temperature range of 300K to 440K, and the color purity of the white long afterglow of the material can also be regulated by temperature in the range of 360K to 380K.
[0147] from Fig.17 It can be seen that the long afterglow material can -2 M), hydrochloric acid (10 -2 M), acetic acid, acetone, acetonitrile (ACN), dichloromethane (DCM), N,N-dimethylformamide (DMF), ethyl acetate (EA), ethanol (EtOH), n-hexane (n-Hexane), tetrahydrofuran (THF), toluene and other common organic solvents, and can still maintain excellent long afterglow luminescence performance.
[0148] from Fig.18 It can be seen that the (I)@PMMA, (I)@PVA, (IV)@PMMA and (IV)@PVA polymer film materials prepared in Comparative Examples 1 to 4 do not have long afterglow luminescence properties, indicating that the long afterglow property of the materials is the effect produced by the interaction between pure hydrocarbon fused ring compounds and melamine formaldehyde resin.
[0149] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A polymer long afterglow material, characterized in that: It comprises a main component and a guest component doped in the main component, wherein the main component is melamine formaldehyde resin, and the guest component is a pure hydrocarbon condensed ring aromatic compound; The pure hydrocarbon fused ring aromatic compound includes one of the compounds of formula (I) to formula (XI): , , , , , , , , , or ; The mass fraction of the guest molecule is 0.001% to 5%.
2. The polymer long afterglow material according to claim 1, characterized in that: The doping includes physical doping.
3. The polymer long afterglow material according to claim 1, characterized in that: The mass fraction of the guest molecule is 0.1%~1%.
4. A method for preparing the polymer long afterglow material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: adding melamine solid and formaldehyde aqueous solution to deionized water, adjusting the pH value of the solution with alkali, and heating to form a mixture solution; S2: adding the organic solution of the pure hydrocarbon condensed ring aromatic compound to the mixed solution, heating for reaction, and then continuing to heat and evaporate the solvent to obtain the polymer long afterglow material; The molar ratio of melamine to formaldehyde is 1:(1-5).
5. The method for preparing the polymer long afterglow material according to claim 4, characterized in that: The molar ratio of melamine to formaldehyde is 1:(2-3).
6. The method for preparing a polymer long afterglow material according to claim 4, characterized in that: The organic solvent of the organic solution includes any one of methanol, ethanol, acetone, N,N-dimethylformamide, tetrahydrofuran or acetonitrile.
7. The method for preparing a polymer long afterglow material according to claim 4, characterized in that: The solution has a pH value of 8-9.
8. A polymer long afterglow film, comprising the polymer long afterglow material according to any one of claims 1 to 3.
9. A method for preparing a polymer long afterglow film as claimed in claim 8, comprising the following steps: The polymer long afterglow material as claimed in any one of claims 1 to 3 is heated and pressed to obtain a polymer long afterglow film.
10. Use of the polymer long afterglow material according to any one of claims 1 to 3 or the polymer long afterglow film according to claim 9 in data encryption and / or anti-counterfeiting and / or functional ink and / or road marking.
Citation Information
Patent Citations
Method for preparing melamine-formaldehyde resin fluorescent microspheres
CN102796512A
Preparation method of organic room-temperature phosphorescent material with ultra-long phosphorescent lifetime
CN114774113A