A preparation method of phenol-biphenylene type epoxy resin
By using proton polar compound additives and alkali-assisted segmented etherification method in the etherification reaction of phenol-biphenyl-biphenyl-type resin, the problem of middle yield and low quality of biphenyl-type epoxy resin is solved, and the problem of low yield and quality of biphenyl-type epoxy resin is achieved. Efficient preparation of epoxy resins has been reduced, and the environmental pressure of environmental pollution and industrial production has been reduced.
Patent Information
- Application Number
- CN202111015316.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-08-31
AI Technical Summary
The use of quaternary ammonium salt catalysts in the synthesis of existing biphenyl epoxy resins results in low yield and quality, and environmental pollution problems, making it difficult to meet the environmental protection requirements of industrial production.
Using proton polar compounds as additives and alkali-assisted etherification reaction methods, the etherification conversion and purity of phenol-biphenyl resins can be improved through segmented etherification and closed-loop reactions, reducing organic chlorine content, and reducing environmental pollution. .
It significantly improves the etherification yield and purity of phenol-biphenylene epoxy resin, reduces the organic chlorine content, relieves environmental protection pressure, and is suitable for industrial production.
Smart Images

Figure BDA0003239758850000031 
Figure BDA0003239758850000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of epoxy resin synthesis, and particularly relates to a phenol-biphenylene epoxy resin and an environmentally friendly preparation method thereof. Background Art
[0002] With the increasingly stringent environmental protection requirements and people's desire for healthy life, the trend of lead-free solder and lead-free electronic products is becoming increasingly urgent. Traditional epoxy resins are facing severe challenges. It is imperative to develop epoxy plastic encapsulation materials with high glass transition temperature, high heat resistance and low water absorption. The biphenyl type epoxy resin structure contains rigid biphenyl ring groups, low melt viscosity, excellent adhesion, flame retardancy, heat resistance, hygroscopicity and other properties. It can be used for lead-free soldering, and the processing temperature is increased from 240℃ of traditional lead-containing solder to 260℃. It is an excellent matrix resin for preparing large-scale and ultra-large-scale integrated circuit packaging materials.
[0003] At present, for the synthesis of biphenyl type epoxy resin, the industry generally adopts quaternary ammonium salt catalyst to catalyze etherification. For example, Japanese Patent Gazette JP2003277468A discloses a method for preparing a biphenyl structure epoxy resin. A quaternary ammonium salt catalyst is used in the preparation process. The quaternary ammonium salt can form ion pairs with tetraalkylammonium ions to form ion pairs with alkali metal hydroxides and inorganic salts that are insoluble in the organic phase, which can easily cause the emulsification of the resin mother liquor and increase the ability of the water phase to dissolve the organic phase, thereby increasing the COD value of the wastewater and aggravating the pollution to the environment.
[0004] In addition, Tan Huaishan et al. also reported the use of quaternary ammonium salt catalyst to synthesize an epoxy resin containing a biphenyl structure, and the product yield was low, at 85%. Chinese patents CN110028652A and CN104004161A also disclose some similar preparation methods.
[0005] In summary, the existing method for synthesizing biphenyl-structured epoxy resins mainly uses quaternary ammonium salt catalysts to catalyze etherification, and the yield and quality of the product need to be further improved. In addition, there is obvious environmental pressure, which is not conducive to actual industrial production. Summary of the invention
[0006] In view of the problems existing in the etherification preparation process of phenol-biphenylene resin, the first purpose of the present invention is to provide an improved etherification method, aiming to solve the technical problems such as large etherification steric hindrance caused by the rigid biphenyl structure in the phenol-biphenylene resin structure, low yield, purity and product quality.
[0007] The second object of the present invention is to provide a method for preparing a phenol-biphenylene epoxy resin, aiming to improve the yield and purity of the product.
[0008] Different from the epoxy etherification of other types of resins, when the rigid biphenyl group in the phenol-biphenylene resin structure is etherified, the steric hindrance is large, and the yield and purity of the product are not high. In view of the difficulty of phenol-biphenylene etherification, the present invention provides the following improvement scheme, specifically:
[0009] A method for epoxy etherification of a phenol-biphenylene resin, comprising subjecting epichlorohydrin, a phenol-biphenylene resin, a base and an auxiliary agent to an etherification reaction;
[0010] The auxiliary agent is a proton polar compound.
[0011] The present invention has found that the etherification is innovatively carried out with the assistance of an auxiliary agent and a base, which can cause the phenol-biphenyl type resin to be in a completely relaxed state, thereby helping to solve the problem of unsatisfactory reaction conversion rate and yield purity caused by the rigidity of the biphenyl, and can significantly improve the etherification yield, purity and quality. In addition, it also alleviates the emission of three wastes, reduces environmental pressure, and is conducive to industrial scale-up.
[0012] In the present invention, the auxiliary agent and the base are the key to improving the etherification effect. The present invention also found that further controlling the composition of the auxiliary agent is helpful to further solve the rigidity defect of biphenyl and help to further improve the etherification effect.
[0013] Preferably, the auxiliary agent is at least one of an alcohol and a polyol ether having a carbon number less than or equal to 10. The alcohol is, for example, a polyol or a monool, and the polyol ether refers to a polyol having two or more ether oxygen atoms. The polyol ether is preferably a linear polyol ether.
[0014] Preferably, the auxiliary agent is one or more of ethylene glycol dimethyl ether, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, propylene glycol methyl ether, dipropylene glycol dimethyl ether, methanol, ethanol, 1-propanol, isopropanol, and n-butanol.
[0015] The auxiliary agent is a combination of a polyol ether and an alcohol. The present invention unexpectedly found through research that the use of the combination of auxiliary agents can unexpectedly achieve synergy, further solve the etherification defects caused by the rigid structure of biphenyl, and improve the etherification reaction effect.
[0016] Preferably, the auxiliary agent accounts for 5-60% of the mass of the epichlorohydrin, preferably 10-40%; more preferably 15-25%.
[0017] In the present invention, the phenol-biphenylene type resin may be a known substance, for example, a substance having a structural formula 1 may be used:
[0018]
[0019] Wherein, n is less than or equal to 10;
[0020] Preferably, the weight ratio of phenol-biphenylene type resin to epichlorohydrin is 1:3-8; more preferably 1:4-5.
[0021] In the present invention, the base is at least one of an alkali metal hydroxide and an alkali metal alkoxide; preferably at least one of sodium hydroxide and potassium hydroxide;
[0022] Preferably, the base is 0.4-3% by weight of the phenol-biphenylene resin; preferably 0.5-1.5%.
[0023] The alkali may be an aqueous solution of alkali, and its concentration is not particularly required. For example, it may be 1 wt % or more to a saturated concentration, and preferably 30 to 40 wt %.
[0024] The segmented etherification treatment with the aid of the auxiliary agent can unexpectedly further improve the synergistic effect of the auxiliary agent and the base, help to further solve the etherification defects caused by the rigid structure of biphenyl, and improve the etherification effect, for example, improve the yield and purity of the etherification.
[0025] Preferably, the alkali is added in N stages, wherein N is greater than or equal to 2, preferably 2 to 5;
[0026] In the present invention, there is no special requirement for the staged addition of the alkali, for example, the amount of the alkali added in each stage is the same or different;
[0027] Preferably, the amount of alkali in each stage is the average amount ± 15 wt %; and the total percentage of alkali added in each stage is equal to 100%. For example, when the alkali is added at both ends, the proportion of alkali added in the first stage is 50-60%.
[0028] In the present invention, the temperature of the etherification reaction is 35-80°C; preferably 45-65°C; and the reaction time is preferably 0.5-5h.
[0029] The present invention also provides a method for preparing a phenol-biphenylene epoxy resin, wherein epichlorohydrin, a phenol-biphenylene resin, a base and an auxiliary agent are subjected to an etherification reaction by the method;
[0030] Then, negative pressure is turned on and alkali is added under reflux to carry out a ring-closing reaction.
[0031] In the present invention, the added base is at least one of an alkali metal hydroxide and an alkali metal alkoxide;
[0032] The amount of the added alkali is 10-40 wt.% of the phenol-biphenylene resin, preferably 20-30 wt.%;
[0033] The additional alkali is added in the form of an aqueous solution, and the concentration of the solution is preferably 30-55%.
[0034] Preferably, during the closed-loop process, the negative pressure is 0.02-0.1 MPa;
[0035] Preferably, the temperature of the ring-closing reaction is 45-85°C, preferably 50-75°C;
[0036] Preferably, the ring-closing reaction time is 3 to 10 hours.
[0037] Preferably, the closed-loop product is recovered, mixed with an alkali solution and a fat-soluble solvent, separated to obtain an oil phase loaded with the product, and then the oil phase is concentrated to obtain a refined phenol-biphenylene epoxy resin;
[0038] Preferably, the base is at least one of an alkali metal hydroxide and an alcoholate;
[0039] Preferably, the fat-soluble solvent is at least one of toluene, ethylbenzene, xylene, methyl ethyl ketone and methyl isobutyl ketone.
[0040] In the present invention, the synthesized phenol-biphenylene epoxy resin has a structural formula of Formula 2, for example.
[0041]
[0042] The present invention discloses a preferred environmentally friendly method for preparing a phenol-biphenylene epoxy resin, comprising the following steps:
[0043] Step (1): First, epichlorohydrin is mixed with an auxiliary agent, and then added to a phenol-biphenylene resin, dissolved at low temperature (dissolution temperature 30-90°C, time 0.5-3h), and alkali solution A is added to carry out etherification reaction; the auxiliary agent is preferably one or more of ethylene glycol dimethyl ether, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, propylene glycol methyl ether, dipropylene glycol dimethyl ether, methanol, ethanol, 1-propanol, isopropanol, and n-butanol. The amount of the auxiliary agent added is 5-60% of the mass of the epichlorohydrin, preferably 10-40%. The etherification reaction temperature is 35-80°C, and the time is 0.5-5h. The temperature is preferably 45-65°C.
[0044] Step (2): Then open the vacuum, add base B under reflux, and carry out ring-closing reaction; after the reaction is completed, recover the excess epichlorohydrin and auxiliary agent, and recycle them; base B is selected from a solution of one or more of sodium hydroxide, potassium hydroxide, and alkali metal alcohol salts, wherein the amount of the base is 10-40% of the phenol-biphenyl type resin. The base B is preferably a 30-55wt.% solution. The ring-closing reaction is carried out at 45-85°C and a negative pressure of 0.02-0.1MPa for 3-10h. The temperature is preferably 50-75°C.
[0045] Step (3): Next, solvent C and base D are added in sequence for refining reaction. After the reaction is completed, the oil phase is taken after washing and layering, and the target product is obtained after desolvation. Solvent C is a non-polar or weakly polar substance, preferably toluene, ethylbenzene, xylene, methyl ethyl ketone, methyl isobutyl ketone, etc. The base D is selected from one or more solutions of sodium hydroxide, potassium hydroxide, and alkali metal alcohol salts, wherein the solid content in the amount of the base is 2 to 8% of the phenol-diphenylene type resin. The preferred concentration is a solution of 10-30%. The refining reaction temperature is 60-100°C and the refining reaction is carried out at normal pressure for 1 to 7 hours. The temperature is preferably 60-80°C. When desolvating, the vacuum degree is -0.02 to -0.1MPa, the final temperature is 130-200°C, and the recovery time is 0.5 to 2h. The vacuum degree is preferably -0.08 to -0.09MPa,
[0046] Beneficial effects:
[0047] 1. The present invention innovatively adopts an auxiliary agent and a base to assist in the etherification reaction, which can achieve synergy and significantly solve the problem of unsatisfactory etherification effect caused by the rigid structure of the phenol-biphenylene resin, and can significantly improve the etherification conversion rate, yield and purity, improve the quality of the product, and reduce the content of organic chlorine;
[0048] For example, the product yield of the present invention is greater than 95%, and the product organic chlorine can be lower than 60ppm, which is far lower than the current industry requirement of 150ppm.
[0049] 2. The combined auxiliary agent can further achieve synergy and improve the effect of the phenol-biphenyl type resin; in addition, the auxiliary segmented etherification process can further improve the etherification effect.
[0050] 3. The preparation process of the present invention has mild conditions and does not use quaternary ammonium salt catalysts in the entire reaction process, which is conducive to industrial production. DETAILED DESCRIPTION
[0051] Phenol-biphenylene resin: Baling Petrochemical, weight average molecular weight (M w ) is between 1200 and 2500 g / mol.
[0052] Yield calculation method: the percentage of actual product mass to theoretical product mass.
[0053] Embodiment 1:
[0054] In a four-mouth round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel, and a condenser, 80 g of phenol-biphenyl resin, 320 g of epichlorohydrin, 40 g of propylene glycol methyl ether, and 24 g of n-butanol were added in sequence and dissolved at 40° C. for 1 hour; the temperature was raised to 55° C., 1 g of 40% sodium hydroxide solution was added, and the reaction was continued for 1 hour. 0.6 g of 40% sodium hydroxide solution was added for the second time, and the reaction was continued for 2 hours; then the vacuum was turned on, the vacuum degree was -0.08 MPa, and 50 % sodium hydroxide solution 45g, the refluxed epichlorohydrin, propylene glycol methyl ether and n-butanol flow back to the reactor in time, and the reaction is maintained for 2 hours; after the reaction is completed, the excess epichlorohydrin and auxiliary agent are removed under reduced pressure, the pressure is -0.09MPa, and the temperature is 130°C; then 600g of methyl isobutyl ketone is added to dissolve the mixture again, and when the temperature reaches 75°C, 10g of 20% sodium hydroxide aqueous solution is added to the formed methyl isobutyl ketone solution, and the reaction is carried out at 75°C for 2 hours. After the reaction is completed, the mixture is washed with deionized water until the water layer is neutral, and the solvent is removed from the oil layer under reduced pressure, the pressure is -0.095, and the temperature is 140°C. A light yellow solid product is obtained. The product yield reaches 98%, the epoxy equivalent is 264g / mol, the total chlorine is 526ppm, and the organic chlorine is 51ppm.
[0055] Embodiment 2: (Compared with Embodiment 1, the only difference is that the mixed auxiliary agent is replaced by a single auxiliary agent.)
[0056] In a four-mouth round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel and a condenser, 80 g of phenol-biphenyl resin, 320 g of epichlorohydrin and 64 g of n-butanol were added in sequence and dissolved at 40 ° C for 1 hour; the temperature was raised to 55 ° C, 1 g of 40% sodium hydroxide solution was added, the reaction was continued for 1 hour, and 0.6 g of 40% sodium hydroxide solution was added for the second time and the reaction was continued for 2 hours; then the vacuum was turned on, the vacuum degree was -0.08 MPa, 45 g of 50% sodium hydroxide solution was added dropwise within 6 hours, and the refluxed epichlorohydrin and n-butanol were promptly returned to the reactor and the reaction was maintained for 2 hours; after the reaction was completed, the excess epichlorohydrin and auxiliary agent were removed under reduced pressure, the pressure was -0.09 MPa, and the temperature was 130 ° C; then 600 g of methyl isobutyl ketone was added to dissolve the mixture again, and when the temperature reached 75 ° C, 10 g of 20% aqueous sodium hydroxide solution was added to the formed methyl isobutyl ketone solution, and the reaction was carried out at 75 ° C for 2 hours. After the reaction was completed, the mixture was washed with deionized water until the water layer was neutral, and the solvent was removed from the oil layer under reduced pressure, pressure -0.095, temperature 140 ° C. A light yellow solid product was obtained. The product yield reached 96%, the epoxy equivalent was 266g / mol, the total chlorine was 570ppm, and the organic chlorine was 53ppm.
[0057] Embodiment 3: (Compared with Embodiment 2, the only difference is that the type of auxiliary agent is changed.)
[0058] In a four-mouth round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel, and a condenser, 80 g of phenol-biphenyl resin, 320 g of epichlorohydrin, and 64 g of ethylene glycol dimethyl ether were added in sequence and dissolved at 40° C. for 1 hour; the temperature was raised to 55° C., 1 g of 40% sodium hydroxide solution was added, and the reaction was continued for 1 hour. 0.6 g of 40% sodium hydroxide solution was added for the second time, and the reaction was continued for 2 hours; then the vacuum was turned on, the vacuum degree was -0.08 MPa, and 50% was added dropwise within 6 hours. 45g sodium hydroxide solution, the refluxed epichlorohydrin and ethylene glycol dimethyl ether flow back to the reactor in time, and the reaction is maintained for 2 hours; after the reaction is completed, the excess epichlorohydrin and auxiliary agent are removed under reduced pressure, the pressure is -0.09MPa, and the temperature is 130°C; then 600g methyl isobutyl ketone is added to dissolve the mixture again, and when the temperature reaches 75°C, 10g 20% sodium hydroxide aqueous solution is added to the formed methyl isobutyl ketone solution, and the reaction is carried out at 75°C for 2 hours. After the reaction is completed, the mixture is washed with deionized water until the water layer is neutral, and the solvent is removed from the oil layer under reduced pressure, the pressure is -0.095, and the temperature is 140°C. A light yellow solid product is obtained. The product yield reaches 96%, the epoxy equivalent is 268g / mol, the total chlorine is 573ppm, and the organic chlorine is 54ppm.
[0059] Example 4: (Compared with Example 1, the only difference is that the method of adding the etherification base is changed from adding in stages to adding in one go.)
[0060] In a four-mouth round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel and a condenser, phenol-biphenyl resin 80g, epichlorohydrin 320g, propylene glycol methyl ether 40g, and n-butyl alcohol 24g were added successively and dissolved at 40 ℃ for 1 hour; the mixture was heated to 55 ℃ and 40% sodium hydroxide solution 1.6g was added and reacted for 3 hours; the vacuum was then opened and the vacuum degree was -0.08MPa. In 6 hours, 45g of 50% sodium hydroxide solution was dripped and the epichlorohydrin, propylene glycol methyl ether and n-butyl alcohol that refluxed were promptly flowed back to the reactor and the reaction was maintained for 2 hours; after the reaction was completed, the excess epichlorohydrin and auxiliary agent were removed under reduced pressure at a pressure of -0.09MPa and a temperature of 130 ℃; 600g of methyl isobutyl ketone was added and the mixture was dissolved again. When the temperature reached 75 ℃, 10g of 20% aqueous sodium hydroxide solution was added to the methyl isobutyl ketone solution formed and the reaction was carried out at 75 ℃ for 2 hours. After the reaction was completed, the mixture was washed with deionized water until the water layer was neutral, and the solvent was removed from the oil layer under reduced pressure, pressure -0.095, temperature 140°C. A light yellow solid product was obtained. The product yield reached 95%, the epoxy equivalent was 268g / mol, the total chlorine was 540ppm, and the organic chlorine was 56ppm.
[0061] Embodiment 5: (Compared with Embodiment 1, the only difference is that the type of auxiliary agent is changed.)
[0062] In a four-necked round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel, and a condenser, 80 g of phenol-biphenyl resin, 320 g of epichlorohydrin, 40 g of diethylene glycol dimethyl ether, and 24 g of isopropanol were added in sequence and dissolved at 40°C for 1 hour; the temperature was raised to 55°C, 1 g of 40% sodium hydroxide solution was added, and the reaction was continued for 1 hour. 0.6 g of 40% sodium hydroxide solution was added for the second time, and the reaction was continued for 2 hours; then the vacuum was turned on, the vacuum degree was -0.08 MPa, and 50% sodium hydroxide solution was added dropwise within 6 hours. 45g of % sodium hydroxide solution, the refluxed epichlorohydrin, diethylene glycol dimethyl ether and isopropanol flow back to the reactor in time, and the reaction is maintained for 2 hours; after the reaction is completed, the excess epichlorohydrin and auxiliary agents are removed under reduced pressure, the pressure is -0.09MPa, and the temperature is 130°C; then 600g of methyl isobutyl ketone is added to dissolve the mixture again, and when the temperature reaches 75°C, 10g of 20% sodium hydroxide aqueous solution is added to the formed methyl isobutyl ketone solution, and the reaction is carried out at 75°C for 2 hours. After the reaction is completed, the mixture is washed with deionized water until the water layer is neutral, and the solvent is removed from the oil layer under reduced pressure, the pressure is -0.095, and the temperature is 140°C. A light yellow solid product is obtained. The product yield reaches 98%, the epoxy equivalent is 264g / mol, the total chlorine is 521ppm, and the organic chlorine is 52ppm.
[0063] Comparative Example 1: (Compared with Example 1, the only difference is that no auxiliary agent is added.)
[0064] In a four-mouth round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel and a condenser, 80 g of phenol-biphenyl resin and 320 g of epichlorohydrin were added in sequence and dissolved at 40 ° C for 1 hour; the temperature was raised to 55 ° C, 1 g of 40% sodium hydroxide solution was added and the reaction was continued for 1 hour, and 0.6 g of 40% sodium hydroxide solution was added for the second time and the reaction was continued for 2 hours; then the vacuum was turned on, the vacuum degree was -0.08 MPa, and 45 g of 50% sodium hydroxide solution was dripped in 6 hours, and the epichlorohydrin, propylene glycol methyl ether and n-butyl alcohol that refluxed flowed back to the reactor in time and maintained the reaction for 2 hours; after the reaction was completed, the excess epichlorohydrin and auxiliary agent were removed under reduced pressure, the pressure was -0.09 MPa, and the temperature was 130 ° C; then 600 g of methyl isobutyl ketone was added to dissolve the mixture again, and when the temperature reached 75 ° C, 10 g of 20% aqueous sodium hydroxide solution was added to the formed methyl isobutyl ketone solution, and the reaction was carried out at 75 ° C for 2 hours. After the reaction was completed, the mixture was washed with deionized water until the water layer was neutral, and the solvent was removed from the oil layer under reduced pressure, pressure -0.095, temperature 140°C. A light yellow solid product was obtained. The product yield reached 79%, the epoxy equivalent was 273 g / mol, the total chlorine was 2400 ppm, and the organic chlorine was 2003 ppm.
[0065] Comparative Example 2: (Compared with Example 2, the only difference is that the type of auxiliary agent is changed, that is, aprotic additives are used.)
[0066] In a four-mouth round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel and a condenser, 80 g of phenol-biphenyl resin, 320 g of epichlorohydrin and 64 g of tetrahydrofuran were added in sequence and dissolved at 40 ° C for 1 hour; the temperature was raised to 55 ° C, 1 g of 40% sodium hydroxide solution was added, the reaction was continued for 1 hour, and 0.6 g of 40% sodium hydroxide solution was added for the second time and the reaction was continued for 2 hours; then the vacuum was turned on, the vacuum degree was -0.08 MPa, 45 g of 50% sodium hydroxide solution was added dropwise within 6 hours, and the refluxed epichlorohydrin and tetrahydrofuran were promptly returned to the reactor and the reaction was maintained for 2 hours; after the reaction was completed, the excess epichlorohydrin and auxiliary agent were removed under reduced pressure, the pressure was -0.09 MPa, and the temperature was 130 ° C; then 600 g of methyl isobutyl ketone was added to dissolve the mixture again, and when the temperature reached 75 ° C, 10 g of 20% aqueous sodium hydroxide solution was added to the formed methyl isobutyl ketone solution, and the reaction was carried out at 75 ° C for 2 hours. After the reaction was completed, the mixture was washed with deionized water until the water layer was neutral, and the solvent was removed from the oil layer under reduced pressure, pressure -0.095, temperature 140°C. A light yellow solid product was obtained. The product yield reached 82%, the epoxy equivalent was 271 g / mol, the total chlorine was 1198 ppm, and the organic chlorine was 579 ppm.
[0067] The above description is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art based on the above description should be included in the protection scope of the present invention. The present invention shall be protected by the scope defined by the attached claims.
Claims
1. A method for preparing a phenol-biphenylene epoxy resin, characterized in that: The steps are: In a four-necked round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel, and a condenser, 80 g of phenol-biphenyl resin, 320 g of epichlorohydrin, 40 g of propylene glycol methyl ether, and 24 g of n-butanol were added in sequence and dissolved at 40°C for 1 hour; the temperature was raised to 55°C, 1 g of 40% sodium hydroxide solution was added, and the reaction was continued for 1 hour. 0.6 g of 40% sodium hydroxide solution was added for the second time, and the reaction was continued for 2 hours; then the vacuum was turned on, the vacuum degree was -0.08 MPa, and 45 g of 50% sodium hydroxide solution was added dropwise within 6 hours. The refluxed epichlorohydrin, propylene glycol methyl ether, and n-butanol were promptly returned to the reactor and the reaction was continued for 2 hours; after the reaction was completed, the pressure was reduced. The excess epichlorohydrin and the auxiliary agent were removed at a pressure of -0.09 MPa and a temperature of 130°C; then 600 g of methyl isobutyl ketone was added to dissolve the mixture again, and when the temperature reached 75°C, 10 g of a 20% aqueous sodium hydroxide solution was added to the formed methyl isobutyl ketone solution, and the reaction was carried out at 75°C for 2 hours; after the reaction was completed, the mixture was washed with deionized water until the water layer was neutral, and the solvent was removed from the oil layer under reduced pressure at a pressure of -0.095 MPa and a temperature of 140°C; a light yellow solid product was obtained; the product yield reached 98%, the epoxy equivalent was 264 g / mol, the total chlorine was 526 ppm, and the organic chlorine was 51 ppm.
2. A method for preparing a phenol-biphenylene epoxy resin, characterized in that: The steps are as follows: in a four-mouth round-bottom flask equipped with a thermometer, a stirrer, a dropping funnel, and a condenser, 80 g of phenol-biphenyl resin, 320 g of epichlorohydrin, 40 g of diethylene glycol dimethyl ether, and 24 g of isopropanol are added in sequence, and dissolved at 40° C. for 1 hour; the temperature is raised to 55° C., 1 g of 40% sodium hydroxide solution is added, and the reaction is continued for 1 hour, and 0.6 g of 40% sodium hydroxide solution is added for the second time, and the reaction is continued for 2 hours; then the vacuum is turned on, the vacuum degree is -0.08 MPa, 45 g of 50% sodium hydroxide solution is added dropwise within 6 hours, and the refluxed epichlorohydrin, diethylene glycol dimethyl ether and isopropanol are promptly returned to the reactor, and the reaction is maintained for 2 hours; the reaction is completed. After that, excess epichlorohydrin and auxiliary agent were removed under reduced pressure at a pressure of -0.09 MPa and a temperature of 130°C; then 600 g of methyl isobutyl ketone was added to dissolve the mixture again, and when the temperature reached 75°C, 10 g of a 20% aqueous sodium hydroxide solution was added to the formed methyl isobutyl ketone solution, and the reaction was carried out at 75°C for 2 hours. After the reaction was completed, the mixture was washed with deionized water until the water layer was neutral, and the solvent was removed from the oil layer under reduced pressure at a pressure of -0.095 MPa and a temperature of 140°C to obtain a light yellow solid product with a product yield of 98%, an epoxy equivalent of 264 g / mol, a total chlorine of 521 ppm, and an organic chlorine of 52 ppm.
Citation Information
Patent Citations
Epoxy resin having biphenyl or polyphenyl structure
CN104004161A
Biphenyl structure containing high-purity epoxy resin and preparation method thereof
CN110028652A
Epoxy resin, epoxy resin composition and its cured product
JP2003277468A
Epoxy resin, curable resin composition, and cured product thereof
CN101291972A
Preparation method of tetramethyl bisphenol F epoxy resin
CN104479105A