A double core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent
Through the dual-core shell magnetic composite magnesium borate microsphere material Fe3O4@SiO2@7MgO·2B2O3·7H2O, using an external magnetic field and functionalization treatment, the problems of difficulty in recycling and insufficient selectivity of traditional magnesium borate adsorbents are solved, and the treatment of large amounts of wastewater is achieved. The efficient adsorption of various pollutants provides an efficient sewage treatment method.
Patent Information
- Application Number
- CN202310016619.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-06
AI Technical Summary
The traditional magnesium borate adsorbent is inconvenient to recycle, suffers quality loss, and has limited adsorption selectivity, which limits its application in wastewater treatment.
The dual-core shell magnetic composite magnesium borate microsphere material Fe3O4@SiO2@7MgO·2B2O3·7H2O is used to separate the solvent and sample through an external magnetic field, and the adsorption performance of different dyes and metal ions is improved through functionalization.
Efficient adsorption of methylene blue and Cu(II) in wastewater is achieved, avoiding the mass loss and selectivity limitations in traditional methods, and providing an efficient adsorbent for sewage treatment.
Smart Images

Figure CN115739053B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorbents, and specifically relates to a double-core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent. Background Art
[0002] Dyes and heavy metal ions in water bodies are considered to be the most basic pollutants that threaten ecological balance and human survival due to their non-biodegradability, toxicity, carcinogenicity and bioaccumulation. Currently, a variety of technologies such as ion exchange, adsorption, membrane filtration, electrochemical treatment and photocatalytic degradation have been developed to remove excessive dyes and heavy metals in wastewater. Among these methods, adsorption is often used as the preferred method for wastewater treatment due to its strong operability, high efficiency, simplicity and low cost. Metal borates have attracted great attention in the selection of adsorbents due to their unique and rich structure and broad research prospects.
[0003] Wancheng Zhu's research group used SiO2 as a template to synthesize uniform mesoporous microspheres Mg3Si2O5(OH)4 as an efficient adsorbent for removing rhodamine B (RhB) (Chinese Journal of Chemical Engineering, 26(2018)1561-1569). Uniform hierarchical porous MgBO2(OH) microspheres prepared by a template-free hydrothermal method had good adsorption properties for Congo red (CR) in simulated wastewater (Chemical Engineering Journal, 334(2018)377-388). Zhihong Liu's research group used a simpler hydrothermal method to prepare hierarchical porous 2MgO·B2O3·H2O microspheres (Journal of theTaiwan Institute of Chemical Engineers, 86(2018)92-100), and prepared hierarchical porous 7MgO·2B2O3·7H2O microspheres through a phase transition of berylite, both of which were used as adsorbents for CR in wastewater (RSC Adv., 9(2019)20009-20018). However, traditional centrifugation or filtration methods severely limit the practical application of magnesium borate, resulting in mass separation loss and morphology damage, which poses a great challenge to the research of magnesium borate. Summary of the invention
[0004] The present invention aims at the disadvantages of traditional magnesium borate adsorbents, such as inconvenient recycling, quality loss, and limited adsorption selectivity. A double-core-shell magnetic composite magnesium borate microsphere material Fe3O4@SiO2@7MgO·2B2O3·7H2O is provided, and the separation of solvent and sample is achieved by applying an external magnetic field; the functionalized Fe3O4@SiO2@7MgO·2B2O3·7H2O-CR is used to remove methylene blue (MB) and Cu(II) in wastewater, and co-adsorption of different dyes and metal ions with good adsorption performance is achieved, which can be used as a promising adsorbent for wastewater treatment.
[0005] The present invention adopts the following technical solution:
[0006] A double core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent, the preparation method of the adsorbent is as follows:
[0007] In the first step, Fe3O4 was added to the isopropanol solution and ultrasonicated for 30 minutes, and then the dispersed solution was transferred to a three-necked volumetric flask and placed in an oil bath at 40 °C for stirring;
[0008] In the second step, 10 mL of ammonia solution and 18 mL of water were slowly dripped in, and after stirring for 30 minutes, 0.5 mL of tetraethyl orthosilicate was quickly injected, and the reaction was continued for 2 hours to obtain a Fe3O4@SiO2 colloidal solution;
[0009] Step 3: PVP and Mg(NO3)2·6H2O were dissolved in deionized water and stirred for 1 hour, then the prepared 0.6 mol / L Na2B4O7·10H2O solution was added dropwise to the mixture and stirred for 3 hours to form a uniform mixed solution and the pH was adjusted to 8;
[0010] Step 4: drop the obtained uniform mixed solution into the above Fe3O4@SiO2 colloidal solution, continue to react and stir for 30 minutes, then transfer all of it into a 100 mL polytetrafluoroethylene autoclave, and react in a constant temperature oven at 60-120°C for 12-48 hours;
[0011] Step 5. After the reaction is completed, the mixture is cooled naturally, and the obtained black precipitate is subjected to magnetic separation, washed with water / ethanol for multiple times, and vacuum dried at 60 °C for 24 hours to obtain the double-core-shell magnetic microsphere adsorbent Fe3O4@SiO2@7MgO·2B2O3·7H2O.
[0012] Fe3O4@SiO2@7MgO·2B2O3·7H2O-CR was obtained after sufficient stirring in Congo red (CR) solution.
[0013] Furthermore, the mass ratio of the PVP to Mg(NO3)2·6H2O is 2:1~8:1.
[0014] Furthermore, the mass ratio of the PVP to Mg(NO3)2·6H2O is 4:1.
[0015] Furthermore, the volume ratio of the deionized water, the Na2B4O7·10H2O solution, and the Fe3O4@SiO2 colloidal solution is 15:1:0.25 to 15:1:2.5.
[0016] Furthermore, the volume ratio of the deionized water, the Na2B4O7·10H2O solution, and the Fe3O4@SiO2 colloidal solution is 15:1:1.25.
[0017] Furthermore, in the fourth step, the reaction temperature is 80° C. and the reaction time is 24 h.
[0018] The beneficial effects of the present invention are as follows:
[0019] The present invention adopts a simple strategy to effectively prepare double core-shell magnetic microspheres Fe3O4@SiO2@7MgO·2B2O3·7H2O, which can achieve separation of solvent and sample by applying an external magnetic field without further centrifugation or filtration. The surface of magnetic nanoparticles is coated with silica, which can alleviate the magnetic dipole and improve biocompatibility, hydrophilicity and chemical stability. In addition, we proposed another strategy to remove MB and Cu(II) from wastewater using functionalized Fe3O4@SiO2@MBH-CR after adsorbing Congo red (CR). Thus, the co-adsorption of different dyes and metal ions with good adsorption properties was successfully achieved, which can be used as a promising adsorbent for wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is the X-ray powder diffraction spectrum of the sample prepared in Example 1.
[0021] Figure 2 It is the Fourier transform infrared spectrum of the sample prepared in Example 1.
[0022] Figure 3 is the SEM image of the sample prepared in Example 1.
[0023] Figure 4 This is the SEM image of the Fe3O4 sample of Comparative Example 1.
[0024] Figure 5 This is the SEM image of Fe3O4@SiO2 in comparative example 2.
[0025] Figure 6This is the SEM image of Comparative Example 3 7MgO·2B2O3·7H2O.
[0026] Figure 7 is the SEM image of the sample prepared in Example 2.
[0027] Figure 8 is the SEM image of the sample prepared in Example 3.
[0028] Fig. 9 Fe3O4, Fe3O4@SiO2, 7MgO·2B2O3·7H2O, and Fe3O4@SiO2@7MgO·2B2O3·7H2O prepared in Example 1;
[0029] Fe3O4@SiO2@7MgO·2B2O3·7H2O prepared in Example 2;
[0030] The Fe3O4@SiO2@7MgO·2B2O3·7H2O prepared in Example 3 adsorbs CR.
[0031] Fig.10 yes
[0032] Fe3O4@SiO2@7MgO·2B2O3·7H2O and Fe3O4@SiO2@7MgO·2B2O3·7H2O-CR adsorb MB and Cu(II). DETAILED DESCRIPTION
[0033] The present invention is further described in conjunction with specific embodiments.
[0034] Example 1
[0035] Add Fe3O4 to the isopropanol solution and ultrasonicate for 30 minutes, then transfer the dispersed solution to a three-necked volumetric flask and place it in an oil bath at 40 °C for stirring;
[0036] 10 mL of ammonia solution and 18 mL of water were slowly dripped in, and after stirring for 30 minutes, 0.5 mL of tetraethyl orthosilicate was quickly injected, and the reaction was continued for 2 hours to obtain a Fe3O4@SiO2 colloidal solution;
[0037] 2.4 g PVP (K30) and 0.6 g Mg (NO3) 2 · 6H2O were dissolved in 60 mL deionized water and stirred for 1 hour. Then 4 mL of 0.6 mol / L Na2B4O7·10H2O solution was added dropwise to the mixture and stirred for 3 hours to form a uniform mixed solution and adjust the pH to 8. The uniform mixed solution was added dropwise to the above 5 mL Fe3O4@SiO2 colloidal solution. After stirring for 30 minutes, it was transferred to a 100 mL polytetrafluoroethylene autoclave and reacted in a constant temperature oven at 80 °C for 24 hours. After natural cooling, the obtained black precipitate was magnetically separated, washed with water / ethanol several times, and vacuum dried at 60 °C for 24 hours to obtain the double core-shell magnetic microsphere adsorbent Fe3O4@SiO2@7MgO·2B2O3·7H2O.
[0038] The inventors used X-ray diffractometer, Fourier transform infrared spectrometer, and cold field emission scanning electron microscope to characterize the magnetic powder obtained in Example 1. Figures 1 to 3 .Depend on Figure 1 XRD and Figure 2 The FT-IR results show that the sample is Fe3O4@SiO2@7MgO·2B2O3·7H2O. Figure 3 contrast Figure 4-6 It can be seen that Fe3O4 is a spherical nanoparticle with a rough surface and an average diameter of about 150 nm ( Figure 4 After being coated with SiO2, the particle surface becomes smooth and forms Fe3O4@SiO2 ( Figure 5 ); After being coated with magnesium borate nanosheets, a multi-level porous flower-like double core-shell Fe3O4@SiO2@7MgO·2B2O3·7H2O was successfully formed ( Figure 3 )
[0039] Comparative Example 1
[0040] Stir 3 g FeCl3·6H2O and 0.8 g Na3C6H5O7·2H2O in 70 mL ethylene glycol for more than 1 hour until all dissolved to form a uniform solution. Quickly add 4.8 g NaAc while stirring continuously and continue stirring for 0.5 hour. The mixture solution is transferred to a polytetrafluoroethylene reactor and reacted at 200 °C for 8 hours. After cooling, place the magnet at a certain height, collect the magnetically attracted substances, pour out the liquid, wash with ethanol and deionized water for several times, and repeat the operation. Dry the product under vacuum at 60 °C for 24 hours to obtain the sample Fe3O4.
[0041] Comparative Example 2
[0042] Fe3O4 was added to the isopropanol solution and ultrasonically treated for 30 minutes. The dispersed solution was then transferred to a three-necked volumetric flask and placed in a 40 °C oil bath for stirring. Subsequently, 10 mL of ammonia solution and 18 mL of water were slowly dripped in. After stirring for 30 minutes, 0.5 mL of tetraethyl orthosilicate (TEOS) was quickly injected and the reaction continued for 2 hours. After washing, magnetic separation, and drying, magnetic Fe3O4@SiO2 powder was obtained.
[0043] Comparative Example 3
[0044] 2.4 g of PVP (K30) and 0.1 g (2.4 mmol) of Mg(NO3)2·6H2O were dissolved in 60 mL of deionized water and stirred for 1 hour, then 4 mL (0.6 mol / L) of Na2B4O7 10·H2O solution was added dropwise to the mixture and continued to stir for 3 hours in a polytetrafluoroethylene high-pressure reactor (100 mL). Finally, it was placed in an oven at 80 °C for 24 hours, cooled naturally, and dried to obtain the sample 7MgO·2B2O3·7H2O.
[0045] Example 2
[0046] 2.4 g PVP (K30) and 0.6 g Mg (NO3) 2 · 6H2O were dissolved in 60 mL deionized water and stirred for 1 hour. Then 4 mL of 0.6 mol / L Na2B4O7·10H2O solution was added dropwise to the mixture and stirred for 3 hours to form a uniform mixed solution and the pH was adjusted to 8. The uniform mixed solution was dropped into the above 1 mL Fe3O4@SiO2 colloidal solution and stirred for 30 minutes. Then, the mixture was transferred to a 100 mL polytetrafluoroethylene autoclave and reacted in a constant temperature oven at 80 °C for 24 hours. After natural cooling, the obtained black precipitate was magnetically separated and washed with water / ethanol several times. The double core-shell magnetic microsphere adsorbent Fe3O4@SiO2@7MgO·2B2O3·7H2O was obtained by vacuum drying at 60 °C for 24 hours.
[0047] Example 3
[0048] 2.4 g PVP (K30) and 0.6 g Mg (NO3) 2 · 6H2O were dissolved in 60 mL deionized water and stirred for 1 hour. Then 4 mL of 0.6 mol / L Na2B4O7·10H2O solution was added dropwise to the mixture and stirred for 3 hours to form a uniform mixed solution and adjust the pH to 8. The uniform mixed solution was added dropwise to the above 10 mL Fe3O4@SiO2 colloidal solution and stirred for 30 minutes. Then, the mixture was transferred to a 100 mL polytetrafluoroethylene autoclave and reacted in a constant temperature oven at 80 °C for 24 hours. After natural cooling, the obtained black precipitate was magnetically separated and washed with water / ethanol several times. The double core-shell magnetic microsphere adsorbent Fe3O4@SiO2@7MgO·2B2O3·7H2O was obtained by vacuum drying at 60 °C for 24 hours.
[0049] Taking CR as the research object, Fe3O4, Fe3O4@SiO2, 7MgO·2B2O3·7H2O, and Fe3O4@SiO2@7MgO·2B2O3·7H2O prepared in Example 1 were added to simulated wastewater to carry out CR adsorption experiments. The results are shown in Fig. 9 The results show that the adsorption performance of the double-core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent prepared in Example 1 of the present invention is better than that of a single sample. The Fe3O4@SiO2@7MgO·2B2O3·7H2O prepared in Example 1 was used to adsorb MB and Cu(II) after adsorbing CR. The adsorption results were compared with those of the Fe3O4@SiO2@7MgO·2B2O3·7H2O in Example 1. Fig.10 The CR-functionalized adsorbent has an ultra-high adsorption capacity. Due to the negative charge modification of the anionic dye CR, the electrostatic effect is enhanced, which significantly improves the adsorption of the cationic dye MB and Cu ions.
Claims
1. A double core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent, characterized in that: The adsorbent can achieve separation of solvent and sample by applying an external magnetic field without further centrifugation or filtration; The preparation method of the adsorbent is as follows: In the first step, Fe3O4 was added to the isopropanol solution and ultrasonicated for 30 minutes, and then the dispersed solution was transferred to a three-necked volumetric flask and placed in an oil bath at 40 °C for stirring; In the second step, 10 mL of ammonia solution and 18 mL of water were slowly dripped in, and after stirring for 30 minutes, 0.5 mL of tetraethyl orthosilicate was quickly injected, and the reaction was continued for 2 hours to obtain a Fe3O4@SiO2 colloidal solution; Step 3: PVP and Mg(NO3)2·6H2O were dissolved in deionized water and stirred for 1 hour, then the prepared 0.6 mol / L Na2B4O7·10H2O solution was added dropwise to the mixture and stirred for 3 hours to form a uniform mixed solution and the pH was adjusted to 8; Step 4: drop the obtained uniform mixed solution into the above Fe3O4@SiO2 colloidal solution, continue to react and stir for 30 minutes, then transfer all of it into a 100 mL polytetrafluoroethylene autoclave, and react in a constant temperature oven at 60-120°C for 12-48 hours; Step 5: After the reaction is completed, the mixture is cooled naturally, and the obtained black precipitate is subjected to magnetic separation, washed with water / ethanol for multiple times, and vacuum dried at 60 °C for 24 hours to obtain the double-core-shell magnetic microsphere adsorbent Fe3O4@SiO2@7MgO·2B2O3·7H2O; Fe3O4@SiO2@7MgO·2B2O3·7H2O-CR was obtained after stirring in a Congo red (CR) solution; after the adsorbent adsorbed Congo red, the functionalized Fe3O4@SiO2@MBH-CR was used to remove MB and Cu(II) in the wastewater, thereby successfully achieving co-adsorption of different dyes and metal ions with good adsorption properties.
2. The double-core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent according to claim 1, characterized in that: The mass ratio of the PVP to Mg(NO3)2·6H2O is 2:1 to 8:
1.
3. The double-core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent according to claim 1, characterized in that: The mass ratio of the PVP to Mg(NO3)2·6H2O is 4:
1.
4. The double-core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent according to claim 1, characterized in that: The volume ratio of the deionized water, the Na2B4O7·10H2O solution and the Fe3O4@SiO2 colloidal solution is 15:1:0.25 to 15:1:2.
5.
5. The double-core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent according to claim 1, characterized in that: The volume ratio of the deionized water, the Na2B4O7·10H2O solution, and the Fe3O4@SiO2 colloidal solution is 15:1:1.
25.
6. The double-core-shell magnetic microsphere Fe3O4@SiO2@7MgO·2B2O3·7H2O adsorbent according to claim 1, characterized in that: In the fourth step, the reaction temperature in the polytetrafluoroethylene high-pressure reactor is 80° C. and the reaction time is 24 h.
Citation Information
Patent Citations
Core-shell nanocomposite as well as preparation method and application thereof
CN113786838A