A kind of nickel-plated cerium dioxide powder and its preparation method and application
By electroless nickel plating on the ceria powder, the problem of insufficient ceria introduction in the nickel-based material is solved, its wetting and density are improved, and the efficient oxidation resistance of the nickel-based composite material is achieved. Improved mechanical performance.
Patent Information
- Application Number
- CN202211467933.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-22
AI Technical Summary
In the prior art, the amount of ceria introduced into nickel-based materials is limited, resulting in the inability to effectively improve its oxidation resistance and mechanical properties. The pressure-free sintering method leads to a decrease in density, making it difficult to meet the demand for increasing nickel or its alloy.
By electroless nickel plating on the surface of ceria powder, the nickel plating layer is activated with silver ammonia solution and the nickel plating layer is deposited on the surface, thereby improving the wettability of nickel to ceria. The nickel-based composite material is added when using the pressure-free sintering method to prepare nickel-based composite material. Nickel ceria is plated to improve its density and oxidation resistance.
It significantly improves the wetting and density of nickel to ceria, extends the application space of ceria in nickel-based materials, reduces the cost of electroless nickel plating process and the difficulty of wastewater treatment, and improves the nickel-based composite materials Antioxidant and density.
Smart Images

Figure CN115740440B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cerium oxide powder surface treatment technology, in particular to a cerium oxide powder surface chemical nickel plating technology. Background Art
[0002] Cerium oxide (CeO2) is a common oxide of the rare earth element cerium. Due to the intrinsic oxygen defects inside, its macroscopic color is light yellow. Its melting point is 2400℃, it has certain oxidizing properties, and it is insoluble in water and alkaline solutions. As a widely used rare earth compound, cerium dioxide has been widely used in solid fuel cells, catalysts, optoelectronic materials, automobile exhaust treatment, biosensors, hydrogen production, etc. This is closely related to the nature of cerium dioxide as an oxygen buffer, that is, cerium dioxide is easy to form surface oxygen defects under real conditions, and the surface oxygen defects of cerium dioxide are easily compounded by oxygen in the air. In addition, cerium dioxide is also one of the rare earth oxides commonly used to improve the oxidation resistance and mechanical properties of metallic nickel and its alloys. The commonly used technical means at present is to introduce cerium dioxide into nickel-based materials by hot pressing sintering, casting and pressureless sintering to improve their oxidation resistance and mechanical properties. Among them, the pressureless sintering method has attracted more attention due to its low cost and simple process. However, due to the poor wettability of metallic nickel on ceria, the introduction of ceria, while improving the oxidation resistance of metallic nickel and its alloys, will cause the density of the composite material to be reduced, which is not conducive to further improving its oxidation resistance. This greatly limits the amount of ceria introduced. This phenomenon is more obvious in the pressureless sintering method, so that the current amount of ceria introduced in the pressureless sintering method is very low, far from meeting the demand for improving the oxidation resistance and mechanical properties of metallic nickel or its alloys. Therefore, how to improve the wettability of metallic nickel on ceria while controlling costs, weaken the effect of introducing ceria on the density reduction of nickel-based composite materials, and further increase the amount of ceria introduced is an urgent technical problem to be solved in this field. At present, there is no feasible solution to this problem. For example, in an article (Effect of nano-CeO2 addition on the consolidation of W-5Ni-3Cu alloy by atwo-step sintering process, Results in Physics, 2019, 15: 102657), the author also found that the introduction of a small amount of ceria is beneficial to the mechanical properties of the metal, and the increase in the amount of ceria introduced reduces the density of the metal, which affects the mechanical properties of the metal. However, the article did not further propose a solution.
[0003] In order to improve this shortcoming, the inventors have found that the surface of the cerium dioxide powder can be modified by plating a layer of metal nickel or alloy layer to improve the wettability of the metal to cerium dioxide. Among them, chemical plating is a method of reducing the target metal ions and depositing them on the surface of the material to form a dense coating by adding a strong reducing agent to a solution containing metal ions based on the principle of redox reaction. This method has the advantages of simple process operation, low cost and good coating performance. At present, chemical nickel plating has the fastest development and the most extensive application. There have been studies on the surface nickel plating of ceramic powders such as SiC and Al2O3, but there has been no report on the research on the surface nickel plating of cerium dioxide powder.
[0004] Although the surface modification of cerium dioxide powder by chemical plating can improve the wettability of metal nickel to cerium dioxide powder, the key to chemical plating process lies in pretreatment. The purpose of pretreatment is to generate metal particles with significant catalytic activity on the surface of the plated part, so that the metal coating can be finally deposited on the surface of the substrate. The activation solutions commonly used in existing chemical plating technology are silver ammonia activation solution and colloidal palladium activation solution. Chemical copper plating is relatively easy, and silver can be used for catalysis. For example, an Al2 In the metallization process of O3 ceramic substrate, when copper is plated on Al2O3 ceramic substrate, silver ammonia solution is directly used for activation and sensitization; while chemical cobalt plating and chemical nickel plating are difficult, silver is not easy to catalyze, and precious metals with strong catalytic properties such as palladium and platinum are generally used for catalysis. For example, a chemical nickel plating method on the surface of micron silicon carbide powder disclosed in Chinese patent CN2013103218831 and the nickel plating technology disclosed in the above CN2013101874605 both use stannous chloride and hydrochloric acid as sensitizers and use metal palladium as an activation solution for catalysis. Due to the use of precious metal palladium, the experimental cost is greatly increased. The introduction of cerium oxide in nickel-based materials is to improve the oxidation resistance of metals. If this purpose is achieved by increasing costs, it is obviously not the right way. Therefore, it is necessary to seek a low-cost and high-efficiency chemical nickel plating method to improve the wettability of nickel to cerium dioxide. Summary of the invention
[0005] In order to increase the amount of cerium dioxide introduced into nickel-based materials to improve the oxidation resistance and weaken the effect of the increased amount on the density of the material, the present invention starts from improving the wettability of nickel on cerium dioxide, thereby providing a nickel-plated cerium dioxide powder.
[0006] The present invention also provides a method for preparing nickel-plated cerium oxide powder with low cost and high nickel plating efficiency, and application of the nickel-plated cerium oxide powder.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] A nickel-plated cerium dioxide powder is characterized in that the cerium dioxide powder after roughening and sensitization is activated by a silver ammonia solution, and then a uniform nickel coating is plated on the surface of the cerium dioxide powder by a chemical plating method. The interface wetting angle between the cerium dioxide and nickel after nickel plating is about 59°, while the wetting angle of nickel to cerium dioxide is about 116°. In comparison, the wettability of nickel to cerium dioxide is significantly improved by nickel plating. When a nickel-based composite material is prepared by a pressureless sintering method, the addition of 1wt% nickel-plated cerium oxide keeps the density of the nickel-based composite material at a high level, and the oxidation resistance of the nickel-based composite material is further improved.
[0009] The method for preparing the nickel-plated cerium dioxide powder comprises the following steps:
[0010] Step 1: Roughening
[0011] The cerium dioxide powder is coarsened by using a hydrochloric acid solution and then washed to neutrality after treatment;
[0012] Step 2: Sensitization
[0013] The roughened cerium dioxide powder is sensitized with stannous chloride and hydrochloric acid solution, and then centrifuged. The purpose of the sensitization treatment is to make the surface of the roughened cerium dioxide powder adsorb a layer of reducing divalent tin ions Sn. 2+ ; so that in the subsequent activation treatment, the silver ions are reduced from metal ions to silver particles with catalytic properties;
[0014] Step 3: Activation
[0015] The sensitized cerium dioxide powder is activated by using a silver ammonia solution prepared by silver nitrate and ammonia water, and then centrifuged and washed to neutrality. The purpose of the activation is to reduce the silver ions in the activation solution to silver with catalytic properties by the divalent tin ions adsorbed on the surface of the cerium dioxide powder;
[0016] Step 4: Prepare chemical nickel plating solution
[0017] The chemical nickel plating solution is placed in a constant temperature water bath and heated to 75-80° C. and kept warm, the activated cerium dioxide powder is added to the constant temperature chemical nickel plating solution, the pH is adjusted to 9-10, the reaction is carried out under stirring until the reaction is completed, and finally washed to neutrality;
[0018] The plating solution contains nickel sulfate as the main salt, sodium citrate as the complexing agent, sodium hydroxide as the buffering agent, and sodium hypophosphite as the reducing agent.
[0019] The principle of chemical plating is to reduce nickel ions to nickel particles through redox reaction between nickel sulfate and sodium hypophosphite, using silver as a catalyst, and deposit them on the surface of cerium dioxide particles to form a dense nickel coating.
[0020] Step 5: centrifuge the solution treated in step 4, wash the lower precipitate to neutrality and dry it at 60° C. to obtain the desired nickel-plated cerium dioxide powder.
[0021] Further: In step 1, the volume concentration of hydrochloric acid is 20%.
[0022] Further: the activation solution-silver ammonia solution is prepared by mixing silver nitrate solution with a concentration of 5g / L and ammonia water.
[0023] Further: the sensitizing solution is composed of 25g / L stannous chloride solution (25g stannous chloride + 1L water) and hydrochloric acid solution with a concentration of 10% (10ml concentrated hydrochloric acid + 90ml water).
[0024] Further: the concentrations of the components of the plating solution after mixing are: nickel sulfate 20-30 g / L, sodium citrate 30-80 g / L, sodium hydroxide 30-50 g / L, sodium phosphite 60-90 g / L.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] 1. In the present invention, for the first time, a cerium dioxide powder with nickel plated on the surface is obtained by chemical plating, which successfully optimizes the wettability of nickel to cerium dioxide, effectively improves the chemical compatibility of cerium dioxide particles and metals, and provides a wider application space for introducing cerium dioxide into metals or composite materials to improve their density. The entire chemical nickel plating process is simple and safe to operate, and the difficulty and cost of wastewater treatment are greatly reduced.
[0027] 2. The present invention uses ammonia water and silver nitrate solution to activate cerium dioxide powder before plating, which is low in cost compared to the existing chemical nickel plating technology that uses palladium chloride for activation treatment; sodium hydroxide is used instead of ammonia water to adjust the pH during the preparation process, firstly, it is avoided that ammonia water volatilizes irritating ammonia gas during the production process, which causes harm to the human body; secondly, ammonia water will accelerate volatilization during the heating process, making it difficult to control the pH of the plating solution. Ammonia water is added in the middle to adjust the pH. Since it takes a certain amount of time for ammonia water to diffuse evenly, the location with high concentration is prone to cause excessively fast local reaction and produce nickel slag. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the description of the specific embodiments will be briefly introduced below. Obviously, the drawings in the following description are some embodiments of the present invention.
[0029] Figure 1 It is a schematic diagram of the chemical nickel plating device of the present invention;
[0030] Figure 2a and 2b A schematic diagram showing a comparison of macroscopic photographs of cerium dioxide powder before and after chemical nickel plating according to the present invention;
[0031] Figure 3a and 3b It is a schematic diagram comparing the microscopic photographs of cerium dioxide powder before and after the chemical nickel plating of the present invention;
[0032] Figure 4a and 4b It is a schematic diagram of the comparison of photographs of the wettability of nickel to cerium dioxide before and after the chemical nickel plating described in the present invention.
[0033] Figure 5 It is a relative density comparison diagram of an embodiment of a TiC / Ni composite material with ceria added and nickel-plated ceria added according to the present invention.
[0034] Figure 6 for Figure 5 A comparison chart of oxidation weight gain of a TiC / Ni composite material to which 0, 0.05wt%, 0.1wt% and 1wt% ceria is added and 1wt% nickel-plated ceria of the present invention is added after oxidation at 800°C for 20h. DETAILED DESCRIPTION
[0035] The technical solution of the present invention will be described below in conjunction with the accompanying drawings. The described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0037] Example 1
[0038] This embodiment provides a method for nickel plating of cerium dioxide powder, which comprises the following steps:
[0039] Step 1: Add cerium dioxide powder to a 20% (volume) hydrochloric acid solution, stir for 15 to 20 minutes, and then perform ultrasonic centrifugation to coarsen the powder. After treatment, wash the powder with plasma water until it is neutral.
[0040] Step 2: Add the coarsened cerium dioxide powder into a mixture of a 25 g / L stannous chloride solution and a 10% by volume hydrochloric acid solution, stir for 15 to 20 minutes, perform ultrasonic centrifugation, and then clean with plasma water.
[0041] Step 3, adding the sensitized cerium dioxide powder into a silver ammonia solution prepared by a silver nitrate solution and ammonia water with a concentration of 5 g / L, stirring for 15 to 20 minutes, ultrasonically centrifuging, and then washing with plasma water;
[0042] Step 4: Prepare a chemical nickel plating solution. When preparing the chemical nickel plating solution, use nickel sulfate with a concentration of 20-30g / L as the main salt, sodium citrate with a concentration of 30-80g / L as the complexing agent, and use a sodium hydroxide solution with a concentration of 30-50g / L to adjust the pH value of the chemical nickel plating solution to 9-10, and use a reducing solution with a sodium hypophosphite concentration of 60-90 / L. Place the chemical nickel plating solution in a constant temperature water bath and heat it to 75-80°C and keep it warm. Add the activated cerium dioxide powder to the constant temperature chemical nickel plating solution, adjust the pH to 9-10, and react under stirring until the reaction is completed;
[0043] Step 5: centrifuge the solution treated in step 4, wash the lower precipitate to neutrality and dry it in a constant temperature drying oven at 60° C. to obtain the desired nickel-plated cerium dioxide powder.
[0044] In the present invention, on the one hand, ammonia water and silver nitrate solution are respectively used to activate the cerium dioxide powder before plating, which is low in cost compared with the activation treatment using palladium chloride in the existing chemical nickel plating technology; on the other hand, sodium hydroxide is used instead of ammonia water to adjust the pH during the preparation process to avoid the use of ammonia water to volatilize irritating ammonia gas during the production process, which causes harm to the human body. In summary, the present invention obtains a nickel-plated cerium dioxide powder with complete, uniform and high purity surface nickel coating by pre-plating treatment, changing the pH regulator and controlling the chemical nickel plating process parameters. The method has low cost and high nickel plating efficiency.
[0045] Figure 1 The device for implementing chemical nickel plating of the present invention comprises a constant temperature magnetic stirrer, a water tank placed on the constant temperature magnetic stirrer for containing chemical nickel plating solution, and a temperature measuring rod; wherein the chemical nickel plating device is mainly used for processing the nickel plating process in step four.
[0046] Example 2
[0047] On the basis of Example 1, this example provides a specific method for nickel plating of cerium dioxide powder, the purpose of which is to chemically plate a uniform nickel coating on 2g of cerium dioxide powder. The specific operation is as follows:
[0048] Step 1: Add 2 g of cerium dioxide powder into 100 mL of roughening solution, wherein the 100 mL of roughening solution is prepared by 20 ml of 37% hydrochloric acid and the remainder of distilled water;
[0049] Step 2: dissolve the cerium dioxide particles roughened in step 1 in 100 ml of a sensitizing solution consisting of stannous chloride and 37% hydrochloric acid, stir at room temperature for 20 minutes, and then wash with deionized water;
[0050] The mass concentration of stannous chloride in the sensitizing solution is 25 g / L, and the volume concentration of HCl is 100 ml / L.
[0051] Step 3: weigh 0.5g of silver nitrate and pour it into a beaker, add water until the solution is 100ml and stir thoroughly, drop ammonia water into the silver nitrate solution to produce a yellow-brown precipitate, then add ammonia water to make the yellow-brown precipitate disappear and make the solution clear; then pour the cerium dioxide particles sensitized in step 2 into the prepared solution, stir for 20 minutes, and wash with deionized water until neutral;
[0052] Step 4: Prepare 200ml of chemical nickel plating solution, wherein the nickel plating solution uses nickel sulfate with a concentration of 30g / L as the main salt, sodium citrate with a concentration of 60g / L as the complexing agent, and then uses a sodium hydroxide solution with a concentration of 50g / L to adjust the pH value of the chemical nickel plating solution to 9-10, and then uses sodium hypophosphite with a concentration of 90g / L to prepare the reducing solution. Pay attention to the order of addition, pour the complexing agent sodium citrate into the nickel sulfate solution while stirring to mix evenly, then pour the reducing agent sodium hypophosphite into the above solution, and then adjust the pH with sodium hydroxide solution. After the nickel plating solution is prepared, pour the pretreated 2g cerium dioxide powder into it, place it in a water bath and heat it to about 80°C, add the rotor, set the speed to start the reaction, and stir for one hour.
[0053] The concentration of each component in the above-mentioned plating solution refers to the concentration of the plating solution after mixing.
[0054] Step 5: subject the solution treated in step 4 to ultrasonic centrifugation, wash the resulting filter residue until it is neutral, and then dry it in a constant temperature drying oven at 60° C. to obtain the desired nickel-plated cerium dioxide powder.
[0055] like Figure 2a-2b As shown in Figures 3a-3b, the macroscopic and microscopic photographs of the nickel-plated cerium dioxide powder (b) prepared in this embodiment and the cerium dioxide powder (a) before nickel plating are compared. It can be seen that the surface of the cerium dioxide particles is evenly coated with a layer of metallic nickel, which can effectively improve the chemical compatibility of the cerium dioxide particles with metals. Figure 4a and 4b The figure shows a comparison of the wettability of nickel to ceria before and after chemical nickel plating. From the comparison results, it can be seen that the interface wetting angle between ceria and nickel after nickel plating is about 59°, while the wetting angle of nickel to ceria is about 116°. In comparison, the wettability of nickel to ceria is significantly improved by nickel plating.
[0056] The nickel-plated cerium oxide powder prepared by the present invention can be used to improve the oxidation resistance of nickel-based composite materials, and the introduction amount can reach 1wt%, and the density of the composite material is still maintained at a high level. In order to verify the advantages of the nickel-plated cerium oxide powder of the present invention in improving the oxidation resistance of nickel-based composite materials, a comparative test is used to illustrate it below.
[0057] The experiment was divided into an experimental group and a control group. Both groups used titanium powder, graphite powder and nickel powder as raw materials (nickel powder mass fraction was 55%, the rest was titanium powder and graphite powder, and the mass ratio of the two was 4:1). The CeO2-TiC / Ni composite material was sintered by pressureless sintering, and the sintering temperature was 1350°C. The experimental group added 0.2wt%, 0.8wt% and 1wt% of nickel-plated cerium dioxide to the composite material, and the control group added 0wt%, 0.05wt%, 0.1wt%, 0.2wt%, 0.8wt% and 1wt% of cerium dioxide to the composite material. The density of the CeO2-TiC / Ni composite materials obtained from the experimental group and the control group was tested and measured respectively. The test results are shown in Figure 5 .from Figure 5 It can be seen that, whether it is the introduction of cerium dioxide or nickel-plated cerium dioxide, as the amount of addition increases, the relative density of the composite material is constantly decreasing, which is an objective existence. However, it is obvious that under the same conditions of the introduction amount, the introduction of nickel-plated cerium dioxide has a much smaller effect on the relative density of the composite material than the non-nickel-plated cerium dioxide. For example, when 1% cerium oxide is added, the relative density of the composite material has dropped to 84.69%, while when 1% nickel-plated cerium oxide is added, the density of the composite material remains at 93.62%. It can also be seen from the curve in the figure that under the same conditions of the relative density of the composite material, the introduction amount of nickel-plated cerium dioxide is much greater than the introduction amount of non-nickel-plated cerium dioxide. For example, when the relative density of the composite material is 93.28%, the introduction amount of non-nickel-plated cerium dioxide is 0.2wt%, while the introduction amount of nickel-plated cerium dioxide is greater than 1wt% at this time.
[0058] In order to verify that the introduction of nickel-plated ceria can further improve the oxidation resistance, the oxidation resistance of CeO2-TiC / Ni composite materials obtained by introducing 0, 0.05wt%, 0.1wt% and 1wt% of unplated nickel ceria in the comparison group and 1wt% of nickel-plated ceria in the test group was tested (800℃, air atmosphere oxidation for 20h). The test results are as follows: Figure 6As shown. As can be seen from the figure, when cerium oxide is not nickel-plated, as the amount of cerium oxide introduced increases, the oxidation weight gain of the composite material decreases, indicating that the antioxidant performance is improved, but when the cerium oxide content is increased to 1wt.%, the oxidation growth increases sharply, indicating that the antioxidant performance is reduced. The reason is that when the amount of cerium oxide introduced is low, the density of the composite material is not significantly affected, but as the cerium oxide content increases, the density of the composite material decreases sharply, thereby further reducing the antioxidant performance of the material. In contrast, by improving the wettability of nickel on cerium dioxide through nickel plating, when 1wt% nickel-plated cerium oxide is introduced into the composite material, the density of the prepared CeO2-TiC / Ni composite material is maintained at 93.62%, the oxidation weight gain of the composite material is significantly lower than the decrease, and the antioxidant performance is significantly improved, and is better than the composite material with 0, 0.05wt% and 0.1wt% cerium oxide added.
[0059] The embodiment of the present invention only studies the effect of nickel-plated cerium oxide on the oxidation resistance of nickel-based composite materials, and does not conduct further research on its mechanical properties and some metals other than nickel. According to the research results in the field on the effect of introducing cerium oxide into metals and their alloys on mechanical properties and oxidation resistance, it can be inferred in principle that the introduction of cerium oxide after nickel plating into some metals and their alloys other than nickel should also have a promoting effect on their oxidation resistance and mechanical properties, and the amount of introduction tends to increase. The specific application is not the focus of the present invention.
[0060] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for applying nickel-plated cerium dioxide powder to improve the oxidation resistance of nickel-based composite materials, characterized in that: The nickel-plated cerium dioxide powder is activated by using a silver ammonia solution to activate the roughened and sensitized cerium dioxide powder, and then a uniform nickel coating is plated on the surface of the cerium dioxide powder by a chemical plating method, and the interface wetting angle between the cerium dioxide and nickel after nickel plating is less than 60°; specifically, the following steps are included: Step 1: Roughening The cerium dioxide powder is coarsened by using a hydrochloric acid solution and then washed to neutrality after treatment; Step 2: Sensitization The roughened cerium dioxide powder is sensitized with stannous chloride and hydrochloric acid solution, and then centrifuged. The purpose of the sensitization treatment is to make the surface of the roughened cerium dioxide powder adsorb a layer of reducing divalent tin ions Sn. 2+ , so that in the subsequent activation treatment, the silver ions are reduced from metal ions to silver particles with catalytic properties; Step 3: Activation The sensitized cerium dioxide powder is activated by using a silver ammonia solution prepared by silver nitrate and ammonia water, and then centrifuged and washed to neutrality. The purpose of the activation is to reduce the silver ions in the activation solution to silver with catalytic properties by the divalent tin ions adsorbed on the surface of the cerium dioxide powder; Step 4: Prepare chemical nickel plating solution The chemical nickel plating solution is placed in a constant temperature water bath and heated to 75-80° C. and kept warm, the activated cerium dioxide powder is added to the constant temperature chemical nickel plating solution, the pH is adjusted to 9-10, the reaction is carried out under stirring until the reaction is completed, and finally washed to neutrality; The plating solution contains nickel sulfate as the main salt, sodium citrate as the complexing agent, sodium hydroxide as the buffering agent, and sodium hypophosphite as the reducing agent. Step 5, centrifuging the solution treated in step 4, washing the lower precipitate to neutrality and drying it at 60° C., thereby obtaining the desired nickel-plated cerium dioxide powder; The application method of the nickel-plated cerium oxide powder in improving the oxidation resistance of nickel-based composite materials is: when preparing TiC / Ni nickel-based composite materials, 1wt% of the nickel-plated cerium oxide powder is introduced into the TiC / Ni nickel-based composite materials, and a pressureless sintering method is adopted to sinter the CeO2-TiC / Ni composite materials; the 1wt% refers to the mass percentage of the nickel-plated cerium oxide powder in the CeO2-TiC / Ni composite materials.
2. The method for applying the nickel-plated cerium dioxide powder to improve the oxidation resistance of nickel-based composite materials according to claim 1, characterized in that: In step 1, the volume concentration of hydrochloric acid is 20%.
3. The method for applying the nickel-plated cerium dioxide powder to improve the oxidation resistance of nickel-based composite materials according to claim 1, characterized in that: The activation solution, silver ammonia solution, is prepared from silver nitrate solution with a concentration of 5g / L and ammonia water.
4. The method for applying the nickel-plated cerium dioxide powder to improve the oxidation resistance of nickel-based composite materials according to claim 1, characterized in that: The sensitizing solution is composed of 25g / L stannous chloride solution and 10% hydrochloric acid solution.
5. The method for applying the nickel-plated cerium dioxide powder to improve the oxidation resistance of nickel-based composite materials according to claim 1, characterized in that: The concentrations of the components of the plating solution after mixing are: 20-30 g / L nickel sulfate, 30-80 g / L sodium citrate, 30-50 g / L sodium hydroxide, and 60-90 g / L sodium phosphite.
Citation Information
Patent Citations
Al3O3 ceramic substrate metallization process
CN103319208A
Method for chemical nickel plating on surface of micron silicon carbide powder
CN103451634A
Modifying method for copper roller face of crystallizer
CN103481025A
In-situ reaction synthesis method of TiC / Ni composite material
CN112899510A
Chemical plating activating process and metal depositing process therewith
CN1740390A