A quartz crucible preparation process for improving transparent layer microbubbles

By adjusting the parameters of mold speed, vacuum degree and arc voltage, the microbubble problem of transparent layer of quartz crucibles is solved, the product quality is significantly improved, and the semiconductor industry's requirements for high purity and transparent layer of quartz crucibles are met.

CN115745382BActive Publication Date: 2024-11-08NINGXIA XINJING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211656768.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-11-08
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

The problem of transparent layer microbubble in the existing quartz crucible preparation process has affected the crystallization rate and quality of silicon ingots, and domestic technology lags behind international levels.

Method used

By adjusting the parameters of mold speed, vacuum degree and arc voltage, the arcing current and vacuum degree are increased by step, forming a sealed liquid phase layer and balancing centrifugal force and gravity, reducing bubble infiltration and vibration, and improving the quality of the transparent layer.

Benefits of technology

The number of micro bubbles in the quartz crucible is significantly reduced, the quality of the transparent layer is improved, the bubbles are prevented from dissolved in the silicon liquid, the liquid level fluctuation and thickness uneven problems are reduced, and the crystallization rate and product quality of single crystal silicon are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115745382B_ABST
    Figure CN115745382B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation process of a quartz crucible, comprising the following steps: placing a quartz sand raw material in a mold, attaching the quartz sand raw material to the inner wall of the mold at a first rotation speed, increasing the arc starting current from zero to the first arc starting current under a first vacuum condition, performing vacuum arc starting melting, and the surface of the quartz sand attached to the inner wall of the mold begins to liquefy and form a sealed liquid phase layer; after the sealed liquid phase layer is formed on the surface of the quartz sand attached to the inner wall of the mold, continuing vacuum arc starting melting under a second vacuum condition, a second rotation speed, and a second arc starting current to prepare a transparent layer of the quartz crucible; and continuing vacuum arc starting melting under a third vacuum condition, a third rotation speed, and a third current to obtain a quartz crucible. The present invention improves the microbubble problem of the transparent layer of the quartz crucible by changing the mold rotation speed, vacuum degree, arc voltage, and other related parameter conditions, thereby reducing the bubble expansion problem in subsequent use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of quartz crucible preparation, and relates to a quartz crucible preparation process, in particular to a quartz crucible preparation process for improving transparent layer microbubbles. Background Art

[0002] With the rapid development of electronic information technology, people's demand for electronic products has gradually increased, and the requirements are getting higher and higher, which has also driven the rapid development of the semiconductor industry. In the semiconductor industry, the purity of single crystal silicon is one of the most important factors affecting the quality of semiconductor products, and it is also one of the most important factors to measure silicon ingots, and the preparation of single crystal silicon ingots at the front end is the top priority. Quartz crucible is one of the most front-end auxiliary products for the production of single crystal silicon ingots, and its product quality is also the most concerned issue for researchers. The product quality of quartz crucible not only includes its appearance and size, but the more important issue is the microbubbles in the transparent layer. Since China started the semiconductor industry later than foreign countries, there is a significant gap. The production of quartz crucibles is also far behind the advanced level of foreign countries. The main reason is that most of the domestic quartz crucible manufacturers often have obvious microbubbles in the transparent layer of the finished quartz crucibles they produce. Especially after use, there is obvious bubble expansion in the transparent layer. This will cause the bubbles in the transparent layer of the quartz crucible to expand and burst during the process of pulling single crystal silicon, which will bring in some impurities into the molten silicon liquid, thereby affecting the crystallization of single crystal silicon and the quality of single crystal silicon.

[0003] Quartz crucible is an indispensable auxiliary product in the process of crystal pulling at the front end of single crystal silicon wafer production. The purity of quartz crucible, transparent layer microbubbles and strength are key factors affecting its preparation. Transparent layer microbubbles are the most basic and important conditions for measuring quartz crucibles. It is not only one of the most basic conditions for a company to gain a foothold in the industry, but also one of the most basic indicators for the company's core technology. Transparent layer microbubbles are mainly composed of crystal water and gas, and the gas composition content is more diverse. In the process of using the crucible, due to the continuous dissolution of silicon liquid on the inner surface in contact with the silicon liquid, and as the microbubbles in the transparent layer continue to grow, the bubbles near the innermost layer will release a certain amount of quartz microparticles and microbubbles when they break. This not only affects the crystallization rate, heating time and cost of silicon, but also affects the quality of single crystal silicon.

[0004] Therefore, how to find a more suitable way to improve the microbubble problem existing in the transparent layer of the existing quartz crucible has become one of the focuses of widespread attention of many forward-looking R&D companies and R&D personnel in the industry. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a quartz crucible preparation process, in particular, a quartz crucible preparation process for improving microbubbles in a transparent layer. The present invention improves the microbubble problem in the transparent layer of the quartz crucible by changing the mold rotation speed, vacuum degree, arc voltage and other related parameter conditions, thereby reducing the bubble expansion problem in subsequent use, and the process is simple and highly controllable, which is more conducive to industrial promotion and application.

[0006] The present invention provides a process for preparing a quartz crucible, comprising the following steps:

[0007] 1) placing a quartz sand raw material in a mold, and at a first rotation speed, the quartz sand raw material adheres to the inner wall of the mold. Under a first vacuum condition, the arc starting current increases from zero to the first arc starting current, and vacuum arc starting melting is performed, and the surface of the quartz sand adhered to the inner wall of the mold begins to liquefy and form a sealed liquid phase layer;

[0008] 2) After a sealed liquid phase layer is formed on the surface of the quartz sand attached to the inner wall of the mold, vacuum arc melting is continued under a second vacuum condition, a second rotation speed, and a second arc current to prepare a transparent layer of the quartz crucible;

[0009] 3) Under the third vacuum condition, the third rotation speed and the third current, the vacuum arc melting is continued to obtain a quartz crucible.

[0010] Preferably, the specific process of increasing the arc starting current from zero to the first arc starting current is: increasing the arc starting current in steps to the first arc starting current;

[0011] The time for the arc starting current to increase from zero to the first arc starting current is 20 to 50 seconds.

[0012] Preferably, the first rotation speed is 75-80 rpm;

[0013] The vacuum degree of the first vacuum is -0.005 to 0.01 MPa;

[0014] The first arc starting current is 4000-4200A.

[0015] Preferably, the time for forming the sealed liquid phase layer is 1 to 3 minutes;

[0016] The thickness of the sealing liquid phase layer is 1 to 3 mm.

[0017] Preferably, the second speed is 76.5-84 rpm;

[0018] The vacuum degree of the second vacuum is -0.01 to 0.1 MPa;

[0019] The second arc starting current is 2000-3000A.

[0020] Preferably, the second speed is greater than the first speed;

[0021] The pressure of the second vacuum is less than the pressure of the first vacuum;

[0022] The second arc striking current is smaller than the first arc striking current.

[0023] Preferably, in step 2), specifically, firstly, the first rotation speed is changed to the second rotation speed, and then the first vacuum and the first arc starting current are changed to the second vacuum and the second arc starting current;

[0024] The thickness of the transparent layer is 2 to 3 mm;

[0025] In the step 2), the time for continuing the vacuum arc melting is 8 to 10 minutes.

[0026] Preferably, the third speed is 78-88 rpm;

[0027] The vacuum degree of the third vacuum is greater than or equal to -0.01 to 0.1 MPa;

[0028] The third arc starting current is 4000-4200A.

[0029] Preferably, the third rotation speed is greater than the second rotation speed;

[0030] The third arc-starting current is greater than the second arc-starting current;

[0031] In the step 3), the vacuum arc melting is continued for 1 to 3 minutes;

[0032] In the step 3), the transparent layer of the quartz crucible is processed to form a layered feeling between the transparent layer and the bubble layer.

[0033] Preferably, the transparent layer continues to be formed during step 3);

[0034] The thickness of the transparent layer formed in step 3) is 1 to 2 mm;

[0035] The inner wall of the mold is provided with a plurality of through holes for vacuuming.

[0036] The invention provides a preparation process of a quartz crucible, comprising the following steps: firstly, placing a quartz sand raw material in a mold; at a first rotational speed, the quartz sand raw material adheres to an inner wall of the mold; under a first vacuum condition, an arc starting current increases from zero to a first arc starting current, vacuum arc starting melting is performed, and the surface of the quartz sand adhered to the inner wall of the mold begins to liquefy and forms a sealed liquid phase layer; then, after the sealed liquid phase layer is formed on the surface of the quartz sand adhered to the inner wall of the mold, vacuum arc starting melting is continued under a second vacuum condition, a second rotational speed and a second arc starting current to prepare a transparent layer of the quartz crucible; finally, under a third vacuum condition, a third rotational speed and a third current, vacuum arc starting melting is continued to obtain the quartz crucible. Compared with the prior art, the present invention aims at the problem of transparent layer microbubbles existing in the existing quartz crucible. The research shows that when the quartz crucible is prepared by the existing quartz crucible vacuum arc method, the mold rotation speed remains unchanged, resulting in a tendency of the silicon liquid on the inner surface to fall, thereby causing the gas to be involved and bubble groups of varying degrees to appear at the R angle, and the too fast electrode arcing also causes the gas to be melted into the silicon liquid before being drawn away in time, thereby increasing the bubble expansion in the later production process. In addition, the vacuum degree that is not a gradient change also affects the increase in the volatility of the silicon liquid level on the inner surface due to excessive vacuum after the quartz sand is melted, which further causes the external gas to be involved in the silicon liquid, affecting the quality of the quartz crucible.

[0037] Based on this, the present invention designs a preparation process of a quartz crucible with specific steps and control methods, which is a quartz crucible preparation process for improving transparent layer microbubbles. Based on the original vacuum arc melting method, the present invention changes certain variables of the prior art. Under the standard of a quartz crucible of a certain size, after adding quartz sand to a metal mold for centrifugal rotation molding, three graphite electrodes start arcing. After arcing in a step-by-step manner to a certain current, its vacuuming also follows the voltage to present a step-by-step frequency conversion. After reaching a certain degree, the existing fixed mold speed is solved, which can no longer meet the balance between silicon liquid and silicon solid. Due to the reduction of friction between them, they will show a certain falling problem. Therefore, the present invention changes the existing mold speed, balances gravity, and on the premise of the previous vacuum balance, raises the vacuum balance point, which not only satisfies the falling of the straight wall quartz sand downward, but also satisfies the dispersion of the horizontal quartz sand to the R angle. The balance between the two makes it just meet the preparation of the quartz crucible. The quartz crucible prepared by the present invention can prevent bubbles from being drawn in by balancing the fluctuation of the quartz liquid level under the centrifugal force, and the wall thickness of each part is relatively uniform. The large vacuum degree can be more conducive to the gas in the quartz sand to be stripped out before it merges into the liquid, so that not only the number of microbubbles before the quartz crucible is used is significantly reduced, but also the expansion of microbubbles in the quartz crucible after use is greatly improved.

[0038] The quartz crucible preparation process provided by the present invention can prevent bubbles from dissolving in silicon liquid, so that the microbubbles in the transparent layer after empty firing are reduced; and because the vacuum degree is small in the early stage, the liquid level fluctuation can be reduced, the inner layer liquid level fluctuation is small, and after solidification, the microbubbles on the surface of the transparent layer are reduced; when the solid state is converted into the liquid state, the mold rotation speed is adjusted to improve the problem of uneven crucible thickness caused by the problem of quartz sand falling due to the imbalance of the balance point between friction and gravity when solid quartz sand is converted into liquid quartz sand; the present invention also adjusts the current gradient and the current size under certain conditions, which can reduce the vibration of quartz sand and effectively reduce the microbubbles in the transparent layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A schematic diagram of the process flow for preparing the quartz crucible provided by the present invention;

[0040] Figure 2 A schematic diagram of the preparation of the quartz crucible provided by the present invention. DETAILED DESCRIPTION

[0041] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.

[0042] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0043] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials of conventional purity used in the field of quartz crucible preparation.

[0044] The present invention provides a process for preparing a quartz crucible, comprising the following steps:

[0045] 1) placing a quartz sand raw material in a mold, and at a first rotation speed, the quartz sand raw material adheres to the inner wall of the mold. Under a first vacuum condition, the arc starting current increases from zero to the first arc starting current, and vacuum arc starting melting is performed, and the surface of the quartz sand adhered to the inner wall of the mold begins to liquefy and form a sealed liquid phase layer;

[0046] 2) After a sealed liquid phase layer is formed on the surface of the quartz sand attached to the inner wall of the mold, vacuum arc melting is continued under a second vacuum condition, a second rotation speed, and a second arc current to prepare a transparent layer of the quartz crucible;

[0047] 3) Under the third vacuum condition, the third rotation speed and the third current, the vacuum arc melting is continued to obtain a quartz crucible.

[0048] The present invention first places a quartz sand raw material in a mold. At a first rotation speed, the quartz sand raw material adheres to the inner wall of the mold. Under a first vacuum condition, an arc starting current increases from zero to a first arc starting current, vacuum arc starting melting is performed, and the surface of the quartz sand adhered to the inner wall of the mold begins to liquefy and form a sealed liquid phase layer.

[0049] In the present invention, the specific process of increasing the arc starting current from zero to the first arc starting current is preferably: increasing the arc starting current to the first arc starting current in steps.

[0050] In the present invention, the time for the arc starting current to increase from zero to the first arc starting current is preferably 20 to 50 s, more preferably 25 to 45 s, and more preferably 30 to 40 s.

[0051] In the present invention, the first rotation speed is preferably 75 to 80 rpm, more preferably 76 to 79 rpm, and more preferably 77 to 78 rpm.

[0052] In the present invention, the vacuum degree of the first vacuum is preferably -0.005 to 0.01 MPa, more preferably -0.004 to 0 MPa, and more preferably -0.003 to -0.002 MPa.

[0053] In the present invention, the first arc starting current is preferably 4000-4200A, more preferably 4040-4160A, and more preferably 4080-4120A.

[0054] In the present invention, the time for forming the sealed liquid phase layer is preferably 1 to 3 minutes, more preferably 1.4 to 2.6 minutes, and more preferably 1.8 to 2.2 minutes.

[0055] After forming a sealed liquid phase layer on the surface of the quartz sand attached to the inner wall of the mold, the invention continues vacuum arc melting under a second vacuum condition, a second rotation speed and a second arc current to prepare a transparent layer of the quartz crucible.

[0056] In the present invention, the second rotation speed is preferably 76.5 to 84 rpm, more preferably 77 to 82 rpm, and even more preferably 79 to 80 rpm.

[0057] In the present invention, the vacuum degree of the second vacuum is preferably -0.01 to 0.1 MPa, more preferably 0.01 to 0.08 MPa, and more preferably 0.03 to 0.06 MPa.

[0058] In the present invention, the second arc starting current is preferably 2000-3000A, more preferably 2200-2800A, and even more preferably 2400-2600A.

[0059] In the present invention, the second rotation speed is preferably greater than the first rotation speed.

[0060] In the present invention, the pressure of the second vacuum is preferably lower than the pressure of the first vacuum.

[0061] In the present invention, the second arc starting current is preferably smaller than the first arc starting current.

[0062] In the present invention, in the step 2), it is particularly preferred that the first rotation speed is first changed to the second rotation speed, and then the first vacuum and the first arc starting current are changed to the second vacuum and the second arc starting current.

[0063] In the present invention, the thickness of the transparent layer is preferably 2 to 3 mm, more preferably 2.2 to 2.8 mm, and more preferably 2.4 to 2.6 mm.

[0064] In the present invention, in the step 2), the time for continuing the vacuum arc melting is preferably 8 to 10 minutes, more preferably 8.4 to 9.6 minutes, and more preferably 8.8 to 9.2 minutes.

[0065] Finally, the present invention continues vacuum arc melting under the third vacuum condition, the third rotation speed and the third current to obtain a quartz crucible.

[0066] In the present invention, the third rotation speed is preferably 78 to 88 rpm, more preferably 80 to 86 rpm, and more preferably 82 to 84 rpm.

[0067] In the present invention, the vacuum degree of the third vacuum is preferably greater than or equal to -0.01 to 0.1 MPa, more preferably 0.01 to 0.08 MPa, and more preferably 0.03 to 0.06 MPa.

[0068] In the present invention, the third arc starting current is preferably 4000-4200A, more preferably 4040-4160A, and more preferably 4080-4120A.

[0069] In the present invention, the third rotation speed is preferably greater than the second rotation speed.

[0070] In the present invention, the third arc striking current is preferably greater than the second arc striking current.

[0071] In the present invention, in the step 3), the time of continuous vacuum arc melting is preferably 1 to 3 minutes, more preferably 1.4 to 2.6 minutes, and more preferably 1.8 to 2.2 minutes.

[0072] In the present invention, in the step 3), it is preferred to process the transparent layer of the quartz crucible so as to form a layered feeling between the transparent layer and the bubble layer.

[0073] In the present invention, it is preferred that the transparent layer continues to be formed during step 3).

[0074] In the present invention, the thickness of the transparent layer formed in step 3) is preferably 1 to 2 mm, more preferably 1.2 to 1.8 mm, and more preferably 1.4 to 1.6 mm.

[0075] In the present invention, the inner wall of the mold preferably has a plurality of through holes for vacuuming.

[0076] In the present invention, the size of the quartz crucible is preferably 28 to 32 inches, more preferably 29 to 31 inches, or 30 inches.

[0077] The present invention believes that under a certain crucible size, the mold speed of the prior art quartz sand centrifugal molding does not take into account that when the quartz sand on the inner surface of the mold is converted into a solid, it can no longer meet the balance of eccentricity and gravity at the current speed, resulting in the fall of a certain amount of quartz sand silicon liquid, which causes the liquid level to fluctuate, and a part of the bubbles are drawn into the transparent layer of the quartz crucible, which also causes the appearance of bubble groups at the R angle. Moreover, for a certain crucible size, the vacuum degree quantitative vacuum pumping speed does not take into account the sharp contrast between the just-molten liquid on the inner surface of the mold and the vacuum pumping speed during the arc starting stage, causing the liquid surface to be turbulent, thereby increasing the amount of bubbles on the surface of the transparent layer, seriously affecting the quality of the quartz crucible, and causing serious adverse effects on the purity of single crystal silicon and crystal pulling. Moreover, the size and change of the graphite electrode voltage greatly affect the quality of the finished quartz crucible. For a certain crucible size, the change in voltage is particularly important. The present invention improves the preparation process of microbubbles in the transparent layer of the quartz crucible, and reasonably adjusts the centrifugal speed, vacuum degree and arc starting current of the mold to a certain extent, thereby intervening in the solidification process of the quartz crucible, which causes the microbubbles in the transparent layer of the quartz crucible to fail to meet the needs of the semiconductor industry due to the unreasonable eccentricity, vacuum degree and current size.

[0078] The present invention is based on the preparation of a quartz crucible with a constant current. The time for the inner surface to become silicon liquid is increased by starting the arc in a step-by-step manner in the early stage, so as to cooperate with vacuuming, thereby reducing the content of bubbles on the surface of the transparent layer. After reaching a suitable solid-liquid conversion state and maintaining it for a certain period of time, the surface is sealed. The current is reduced in a step-by-step manner, and after it drops to a certain current, it is kept constant for a long time, so that the gas has sufficient time to be discharged, and the silicon liquid can also be prevented from dissolving the gas. When the transparent layer that meets the requirements is reached, the current is increased in a step-by-step manner for a short time, and the voltage is turned off to obtain the transparent layer.

[0079] See also Figure 1 , Figure 1 The present invention provides a schematic diagram of the process flow for preparing a quartz crucible.

[0080] See also Figure 2 , Figure 2This is a schematic diagram of the preparation of the quartz crucible provided by the present invention. 1 is a high-purity graphite electrode; 2 is a mold liner; 3 is a mold vacuum hole; 4 is a quartz crucible bubble layer; 5 is a quartz crucible transparent layer.

[0081] Figure 1 The paper briefly describes the changes in mold speed, vacuum and current during the growth of the transparent layer in each time period when preparing the quartz crucible. The conditions before the transparent layer are to reduce the fluctuation of the liquid level in the inner layer of the quartz crucible and reduce the bubbles on its surface; the middle layer of the transparent layer is to prevent the bubbles from dissolving in the liquid and the silicon liquid from falling as much as possible; the end of the transparent layer is the finishing stage, and the short-term finishing with high current, high vacuum and high speed is to achieve the interface bonding between the bubble composite layer and the transparent layer.

[0082] The present invention adopts the method of changing the mold rotation speed to obtain a mold rotation speed that is more suitable for the solid and liquid phases of quartz sand. The step-by-step vacuuming is adopted in the early stage of vacuuming. When a certain vacuum degree is reached, a constant pumping speed is performed. When the liquid level saturation is reached, the vacuum degree is increased on this basis to vacuumize until a suitable transparent layer is formed. The step-by-step increase of the current can appropriately reduce the vibration of the quartz sand. After a period of constant current, the current is reduced, so that there is sufficient time to ensure that the transparent layer removes excess air.

[0083] The above content of the present invention provides a quartz crucible preparation process for improving transparent layer microbubbles. Based on the original vacuum arc melting method, the present invention changes certain variables of the prior art. Under the standard of a quartz crucible of a certain size, after adding quartz sand into a metal mold for centrifugal rotation molding, three graphite electrodes start arcing. After arcing in a step-by-step manner to a certain current, the vacuuming also shows a step-by-step frequency conversion following the voltage. After reaching a certain degree, the existing fixed mold speed is solved, which can no longer meet the balance between silicon liquid and silicon solid. Due to the reduction of friction between them, they will show a certain falling problem. Therefore, the present invention changes the existing mold speed, balances gravity, and on the premise of the previous vacuum balance, raises the vacuum balance point, which not only satisfies the falling of the straight wall quartz sand, but also satisfies the dispersion of the horizontal quartz sand to the R angle. The balance between the two makes it just meet the preparation of the quartz crucible. The quartz crucible prepared by the present invention can prevent bubbles from being drawn in by balancing the fluctuation of the quartz liquid level under the centrifugal force, and the wall thickness of each part is relatively uniform. The large vacuum degree can be more conducive to the gas in the quartz sand to be stripped out before it merges into the liquid, so that not only the number of microbubbles before the quartz crucible is used is significantly reduced, but also the expansion of microbubbles in the quartz crucible after use is greatly improved.

[0084] The quartz crucible preparation process provided by the present invention can prevent bubbles from dissolving in silicon liquid, so that the microbubbles in the transparent layer after empty firing are reduced; and because the vacuum degree is small in the early stage, the liquid level fluctuation can be reduced, the inner layer liquid level fluctuation is small, and after solidification, the microbubbles on the surface of the transparent layer are reduced; when the solid state is converted into the liquid state, the mold rotation speed is adjusted to improve the problem of uneven crucible thickness caused by the problem of quartz sand falling due to the imbalance of the balance point between friction and gravity when solid quartz sand is converted into liquid quartz sand; the present invention also adjusts the current gradient and the current size under certain conditions, which can reduce the vibration of quartz sand and effectively reduce the microbubbles in the transparent layer.

[0085] In order to further illustrate the present invention, the preparation process of a quartz crucible provided by the present invention is described in detail below in combination with examples. However, it should be understood that these examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention. The protection scope of the present invention is not limited to the following examples.

[0086] Example

[0087] The preparation process of this experimental scheme is as follows: in the first stage: time 0-30s, mold speed 76rpm, vacuum 25Hz, and current step-by-step increase to 4000A; then the second stage: time 30s-2min45s, mold speed 78rpm, vacuum 50Hz, and constant current 3000A; the last stage: time 2min45s-3min, mold speed 81rpm, vacuum 50Hz, and constant current 4000A.

[0088] See Table 1, which is a data comparison of the quartz crucible prepared by the embodiment of the present invention and the quartz crucible prepared by the existing vacuum arc melting process.

[0089] Table 1

[0090]

[0091] The above is a detailed introduction to a quartz crucible preparation process for improving transparent layer microbubbles provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified in several ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the text of the claims, or if they include equivalent structural elements that are not substantially different from the text of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A process for preparing a quartz crucible, characterized in that: The following steps are involved: 1) Put the quartz sand raw material in the mold. At the first rotation speed, the quartz sand raw material adheres to the inner wall of the mold. Under the first vacuum condition, the arc starting current increases from zero to the first arc starting current, and vacuum arc starting melting is performed. The surface of the quartz sand adhered to the inner wall of the mold begins to liquefy and form a sealed liquid phase layer. The time for the arc starting current to increase from zero to the first arc starting current is 20 to 50 seconds; The first arc starting current is 4000~4200A; The specific process of increasing the arc starting current from zero to the first arc starting current is: increasing the arc starting current step by step to the first arc starting current; The first rotation speed is 75-80 rpm; The thickness of the sealing liquid phase layer is 1-3 mm; The vacuum degree of the first vacuum is -0.005~0.01MPa; 2) After a sealed liquid phase layer is formed on the surface of the quartz sand attached to the inner wall of the mold, vacuum arc melting is continued under the second vacuum condition, the second rotation speed and the second arc current to prepare a transparent layer of the quartz crucible; The second speed is 76.5~84rpm; The second rotation speed is greater than the first rotation speed; The pressure of the second vacuum is less than the pressure of the first vacuum; The second arc starting current is smaller than the first arc starting current; The second arc starting current is 2000~3000A; The vacuum degree of the second vacuum is -0.01~0.1MPa; In the step 2), specifically, the first rotation speed is first changed to the second rotation speed, and then the first vacuum and the first arc starting current are changed to the second vacuum and the second arc starting current; The thickness of the transparent layer is 2-3 mm; 3) Under the third vacuum condition, the third rotation speed and the third arc starting current, the vacuum arc starting and melting are continued to obtain a quartz crucible; The third rotation speed is 78-88 rpm; The third arc starting current is 4000~4200A; The third rotation speed is greater than the second rotation speed; The third arc-starting current is greater than the second arc-starting current; The vacuum degree of the third vacuum is greater than or equal to -0.01~0.1MPa; In the step 3), the transparent layer of the quartz crucible is processed to form a layered feeling between the transparent layer and the bubble layer; During the step 3), a transparent layer continues to be formed; The thickness of the transparent layer formed in step 3) is 1-2 mm.

2. The preparation process according to claim 1, characterized in that: The time for forming the sealed liquid phase layer is 1 to 3 minutes.

3. The preparation process according to claim 1, characterized in that: In the step 2), the time for continuing the vacuum arc melting is 8 to 10 minutes.

4. The preparation process according to claim 1, characterized in that: In the step 3), the vacuum arc melting is continued for 1 to 3 minutes.

5. The preparation process according to claim 1, characterized in that: The inner wall of the mold is provided with a plurality of through holes for vacuuming.