Porous water-absorbing resin, preparation method thereof, sanitary products, water-retaining agent, and waterproof coating

By designing water-absorbent resin with a porous structure and utilizing hydrophilic groups and dehydration pore-forming reactions, the problem of insufficient water absorption speed and amount of water-absorbent resin is solved, achieving more efficient water absorption and permeability, and reducing surface agglomeration.

CN115746483BActive Publication Date: 2024-10-29GUANGZHOU TONGFUGUI CHEM CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211579327.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-10-29
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

The water absorption speed and water absorption capacity of existing water-absorbent resins need to be improved, which results in their slow water absorption speed and reduced water absorption capacity in application, and they are prone to surface caking, preventing water from continuing to penetrate.

Method used

Using the design of porous water-absorbent resin, the polymer of ethylenically unsaturated monomers containing hydrophilic groups is used to form a surface porous structure, and combined with dehydration pore-forming reaction and surface cross-linking reaction, a pore size of 0.5 to 2 microns is formed to improve water penetration. and water-absorbing properties.

Benefits of technology

It significantly increases the water absorption speed and amount, slows down surface agglomeration, and enhances the fluidity of water inside the resin. It performs better than non-porous particles or grape bunch-shaped particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115746483B_ABST
    Figure CN115746483B_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of water-absorbing resins, and in particular relates to a porous water-absorbing resin and a preparation method thereof, as well as sanitary products, water-retaining agents, and waterproof coatings; the porous water-absorbing resin is a polymer of an ethylenically unsaturated monomer containing a hydrophilic group, which can slow down the agglomeration of the surface of the water-absorbing resin, increase the water absorption speed and water absorption amount, thereby solving the technical problem in the prior art that the water absorption speed and water absorption amount of the water-absorbing resin need to be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of water-absorbing resins, and in particular relates to a porous water-absorbing resin and a preparation method thereof, as well as sanitary products, a water-retaining agent, and a waterproof coating. Background Art

[0002] Unlike traditional water-absorbing materials such as sponges, water-absorbing resin, as a polymer material containing a large number of hydrophilic groups, can absorb dozens or even thousands of times its own weight of water. Therefore, it can be used in daily necessities such as diapers, planting fields such as water-retaining materials, and industrial fields such as anti-condensation materials.

[0003] At present, water-absorbent resins are usually spherical particles with a wide particle size distribution. Among the water-absorbent resin spherical particles with a high particle size distribution, small-sized water-absorbent resin particles are easily filled between large-sized water-absorbent resin particles, resulting in small gaps between the water-absorbent resin spherical particles. After absorbing water, the surface agglomerates, preventing water from continuing to penetrate into the lower layer, causing the water-absorbent resin spherical particles to absorb water slowly and reduce the amount of water absorbed. In order to increase the gaps between the water-absorbent resin particles and improve the water absorption performance of the water-absorbent resin, Sumitomo Chemical provides a "grape bunch" shaped water-absorbent resin particle, in which individual spherical particles are bonded to each other to form "grape bunch" shaped particles of a certain particle size, thereby increasing the gaps between the "grape bunch" particles and the spherical particles inside them, which is beneficial for water to penetrate into the lower layer and increase the water absorption rate. However, when the "grape bunch" shaped water-absorbent resin particles absorb water, they still need to rely on the gaps between the water-absorbent resin particles to allow water to penetrate downward, and the water absorption rate and amount of the water-absorbent resin spherical particles need to be improved. Summary of the invention

[0004] In view of this, the present application provides a porous water-absorbing resin and a preparation method thereof, as well as sanitary products, a water-retaining agent, and a waterproof coating, which are used to solve the technical problem in the prior art that the water absorption speed and water absorption amount of the water-absorbing resin need to be improved.

[0005] In a first aspect, the present application provides a porous water-absorbent resin, wherein the porous water-absorbent resin is a polymer of an ethylenically unsaturated monomer containing a hydrophilic group;

[0006] The polymer of the ethylenically unsaturated monomer containing a hydrophilic group has a surface porous structure.

[0007] Preferably, the polymer of the ethylenically unsaturated monomer containing a hydrophilic group is acrylate, polyvinyl alcohol or a copolymer thereof.

[0008] Preferably, the pore size of the polymer of the ethylenically unsaturated monomer containing a hydrophilic group is 0.5 to 2 microns.

[0009] The second aspect of the present application provides a method for preparing a porous water-absorbing resin, the preparation method comprising the steps of:

[0010] Step S1, dissolving an ethylenically unsaturated monomer containing a hydrophilic group, an initiator, a crosslinking agent, and a porogen in an aqueous solution of sodium hydroxide to obtain a solution to be polymerized;

[0011] Step S2, mixing the solution to be polymerized, a hydrocarbon dispersant, and a dispersion stabilizer, and performing a polymerization reaction to obtain a polymer suspension of an ethylenically unsaturated monomer containing a hydrophilic group;

[0012] Step S3, heating the polymer suspension of the ethylenically unsaturated monomer containing a hydrophilic group to perform a dehydration pore-forming reaction to obtain a dehydrated porous water-absorbing resin;

[0013] Step S4: mixing the dehydrated porous water-absorbent resin with a surface cross-linking agent to carry out a surface cross-linking reaction to obtain a porous water-absorbent resin.

[0014] Preferably, in step S1, the porogen is bicarbonate, and in step S3, the temperature of the dehydration pore-forming reaction is 120°C.

[0015] Preferably, the bicarbonate is any one or at least two of sodium bicarbonate, potassium bicarbonate, and calcium bicarbonate.

[0016] Preferably, in step S1, the hydrophilic group-containing ethylenically unsaturated monomer includes any one or at least two of acrylic acid, methacrylic acid, acrylamide, and methacrylamide.

[0017] Preferably, in step S1, the initiator includes any one or at least two of potassium persulfate, ammonium persulfate, and sodium persulfate.

[0018] Preferably, in step S1, the cross-linking agent includes any one or at least two of N,N-methylenebisacrylamide, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, and glycerol diglycidyl ether.

[0019] Preferably, in step S2, the hydrocarbon dispersant includes any one or at least two of n-hexane, n-heptane, cyclohexane, cyclopentane, benzene, toluene and xylene.

[0020] Preferably, in step S2, the dispersion stabilizer includes any one or at least two of sorbitan fatty acid ester, polyglycerol fatty acid ester, and sucrose fatty acid ester.

[0021] Preferably, in step S2, the polymerization reaction is carried out at a temperature of 60 to 80° C. and for a time of 1 to 2 hours.

[0022] Preferably, in step S3, the water content of the dehydrated porous water-absorbing resin is less than 30%.

[0023] Preferably, in step S4, the surface cross-linking reaction is carried out at a temperature of 70 to 90° C. and for a time of 1 to 2 hours.

[0024] Preferably, in step S4, the surface cross-linking agent includes ethylene glycol diglycidyl ether.

[0025] The third aspect of the present application provides a sanitary product, characterized in that it comprises an inner layer, an outer layer and the above-mentioned porous water-absorbing resin;

[0026] The porous water-absorbing resin is wrapped by an inner layer and an outer layer.

[0027] The fourth aspect of the present application provides a water-retaining agent, characterized in that it includes the above-mentioned porous water-absorbing resin.

[0028] The fifth aspect of the present application provides a waterproof coating, characterized in that it includes a film-forming component, a solvent and the above-mentioned porous water-absorbing resin.

[0029] In summary, the present application provides a porous water-absorbent resin and a preparation method thereof, as well as sanitary products, water-retaining agents, and waterproof coatings; the porous water-absorbent resin is a polymer of an ethylenically unsaturated monomer containing a hydrophilic group, and has a porous structure. The hydrophilic group can adsorb water molecules, so that the polymer of the ethylenically unsaturated monomer has water-absorbing properties, and the porous structure forms pores extending to the inside, which is conducive to the flow of water inside the water-absorbent resin. Compared with non-porous particles or grape bunch water-absorbent resins, the water-absorbent resin surface agglomeration can be slowed down, thereby increasing the water absorption speed and the water absorption amount, thereby solving the technical problem in the prior art that the water absorption speed and water absorption amount of the water-absorbent resin need to be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0031] Figure 1 This is a scanning electron microscope image of the porous water-absorbent resin provided in Example 1 of the present application. DETAILED DESCRIPTION

[0032] The present application provides a porous water-absorbing resin and a preparation method thereof, as well as sanitary products, a water-retaining agent, and a waterproof coating, which are used to solve the technical problem in the prior art that the water absorption speed and water absorption amount of the water-absorbing resin need to be improved.

[0033] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0034] Example 1

[0035] This embodiment provides a porous water-absorbing resin, and its microstructure is shown in the attached Figure 1 The porous water-absorbent resin is a polymer of ethylenically unsaturated monomers containing hydrophilic groups; the polymer of ethylenically unsaturated monomers containing hydrophilic groups has a surface porous structure, and the hydrophilic groups in the polymer of ethylenically unsaturated monomers containing hydrophilic groups can adsorb water molecules, thereby making the polymer of ethylenically unsaturated monomers have water-absorbing properties, and the porous structure forms pores extending to the interior, which is conducive to the flow of water inside the water-absorbent resin. Compared with non-porous particles or grape bunch water-absorbent resins, it can slow down the surface agglomeration of the water-absorbent resin surface, thereby increasing the water absorption speed and the water absorption amount.

[0036] For the specific type of polymer of ethylenically unsaturated monomer containing hydrophilic group, acrylate, polyvinyl alcohol or copolymer of the two can be selected. The hydroxyl groups contained in acrylate, polyvinyl alcohol or copolymer of the two can absorb water molecules, thereby giving the polymer of ethylenically unsaturated monomer containing hydrophilic group water absorption property.

[0037] Example 2

[0038] This embodiment 2 provides a method for preparing the porous water-absorbent resin described in embodiment 1, the preparation method comprising the steps of preparing a solution to be polymerized, a polymerization reaction, a dehydration pore-forming reaction, and a surface cross-linking reaction.

[0039] The steps of preparing the solution to be polymerized include weighing 45g of an ethylenically unsaturated monomer acrylic acid containing a hydrophilic group, adding 11.25g of water to dilute it, dripping 83.3g of a 30% by mass NaOH solution into an acrylic acid aqueous solution under ice-water bath conditions, stirring until the solution is transparent and no precipitation is precipitated, adding 0.0675g of an initiator potassium persulfate, 0.0112g of a cross-linking agent N,N-methylenebisacrylamide, and then adding 1.8g of a porogen sodium bicarbonate, mixing and stirring to obtain a solution to be polymerized.

[0040] The polymerization reaction steps include adding 180g of hydrocarbon dispersant n-heptane and 0.59g of dispersant sucrose fatty acid ester into a four-necked flask equipped with a stirring paddle, a thermometer and a reflux condenser, stirring, heating to 70°C until the sucrose fatty acid ester is completely dissolved, adding the prepared sodium acrylate aqueous solution, passing nitrogen, stirring at a speed of 350r / min, and keeping the temperature at 70°C for 1-2h to initiate polymerization of sodium acrylate, then heating to 80°C and keeping the temperature for 1h to complete the reaction of sodium acrylate to obtain a polymer suspension of ethylenically unsaturated monomers containing hydrophilic groups.

[0041] The dehydration pore-forming reaction step includes heating a polymer suspension of an ethylenically unsaturated monomer containing a hydrophilic group to 120° C. to separate water from particles, while high temperature accelerates the decomposition of sodium bicarbonate to generate carbon dioxide, forming a porous structure inside the particles, and the solvent flows back into the reactor. When the water content in the particles is reduced to below 30%, the separation is terminated to obtain a dehydrated porous water-absorbing resin.

[0042] The step of surface crosslinking reaction includes adding 1.2g of surface crosslinking agent (ethylene glycol diglycidyl ether), and performing surface crosslinking reaction at 80°C for 1h until the reaction is complete. The mixture is cooled to room temperature, filtered, and the filter cake is collected as porous water-absorbing resin particles. After the surface crosslinking reaction, the surface crosslinking degree of the dehydrated porous water-absorbing resin is increased, which is beneficial to increasing the hardness of the surface of the porous water-absorbing resin, slowing down the surface agglomeration caused by the surface water absorption and swelling of the porous water-absorbing resin, and preventing water from continuing to penetrate into the lower layer.

[0043] Example 3

[0044] This Example 3 provides a method for preparing the porous water-absorbent resin described in Example 1. The difference between the preparation method and Example 2 is that the amount of the porogen sodium bicarbonate is reduced to 0.6 g.

[0045] Example 4

[0046] This Example 4 provides a method for preparing the porous water-absorbent resin described in Example 1. The difference between the preparation method and Example 2 is that the amount of the porogen sodium bicarbonate is increased to 3.6 g.

[0047] Example 5

[0048] This embodiment provides a method for preparing a water-absorbing resin. The difference between the preparation method and the embodiment 2 is that the porogen sodium bicarbonate is not added.

[0049] Example 6

[0050] This embodiment provides a sanitary product, which includes an inner layer, an outer layer, and a porous water-absorbing resin wrapped in the inner and outer layers.

[0051] The sanitary products can be baby diapers, adult diapers and sanitary napkins for women. The structure of the sanitary products is the conventional structure currently available on the market. The inner and outer layers of the sanitary products are made of existing materials on the market, and the porous water-absorbent resin wrapped in the inner and outer layers is the porous water-absorbent resin provided in Examples 2-4 of the present application.

[0052] Example 7

[0053] This embodiment provides a water-retaining agent, which is the porous water-absorbing resin provided in Examples 2-4 of the present application.

[0054] The water retaining agent can be a water retaining agent for various crops and ornamental plants. When in use, the porous water-absorbing resin water retaining agent can be buried in the roots of crops and ornamental plants. After absorbing water, the water retaining agent plays a water-slow-release effect, thereby improving water utilization efficiency.

[0055] Example 8

[0056] This embodiment provides a waterproof coating, characterized in that it includes a film-forming component, a solvent, and the porous water-absorbing resin provided in Examples 2-4 of the present application.

[0057] The film-forming component and solvent in the composition of the waterproof coating are conventional components of coatings on the market, and the porous water-absorbing resin provided in Examples 2-4 of the present application is added to the coating as an auxiliary agent to give the coating a waterproof function. When the waterproof coating is used, it can be applied in the storage room and coated on the walls of the storage room to absorb moisture and prevent condensation on the walls, thereby maintaining a dry environment in the storage room; it can also be coated on the surface of the cable to absorb moisture and slow down the penetration of external moisture into the conductor inside the cable.

[0058] Test Example 1

[0059] This test example is used to test the water absorption speed and water absorption amount of the porous water-absorbing resin, water-absorbing resin and Sumitomo 60S super absorbent resin provided in Examples 2-5; the test results are shown in Table 1.

[0060] Among them, the water absorption speed test process is to add 1g of the porous absorbent resin, water absorbent resin and Sumitomo 60S super absorbent resin provided in Examples 2-5 into 100g of distilled water, and record the time when all the water is absorbed. The water absorption amount test process is to add 1g of the porous absorbent resin, water absorbent resin and Sumitomo 60S super absorbent resin provided in Examples 2-5 into 1000g of distilled water, let it stand for 1h, filter with a filter bag, and weigh the weight of the resin after water absorption.

[0061] Water absorption speed / s Water absorption / g Example 2 25s 530g Example 3 48s 320g Example 4 36s 360g Example 5 90s 300g Sumitomo 60s 29s 380g

[0062] Table 1

[0063] It can be seen from Table 1 that 1g of the water-absorbent resin provided in Example 5 takes 90s to absorb 100g of distilled water, and the final water absorption is 300g, while 1g of the porous water-absorbent resin provided in Examples 2-4 only takes 25-48s to absorb 100g of distilled water, and the final water absorption is 320-530g. This shows that the porous structure in the porous water-absorbent resin provided in the present application forms pores extending to the inside, which is conducive to the flow of water inside the water-absorbent resin. Compared with the non-porous water-absorbent resin, it can slow down the surface agglomeration of the water-absorbent resin surface, thereby increasing the water absorption speed and the water absorption amount.

[0064] At the same time, the water absorption speed and water absorption capacity of the porous water absorbent resin provided in Example 3 are lower than those of the porous water absorbent resins provided in Examples 2 and 4. This is because the amount of porogen used in Example 3 is too small, and the pores generated inside the porous water absorbent resin particles are relatively small, which cannot achieve the purpose of rapid water absorption. The water absorption speed and water absorption capacity of the porous water absorbent resin provided in Example 4 are lower than those of the porous water absorbent resin provided in Example 2. This is because when the amount of porogen used is too large, more gas is generated by decomposition, and gas agglomeration is likely to occur. The pore structure size and distribution of the obtained porous water absorbent resin are very uneven, which reduces the water absorption performance of the porous water absorbent resin.

[0065] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A porous water-absorbing resin, characterized in that: The porous water-absorbing resin is a polymer of an ethylenically unsaturated monomer containing a hydrophilic group; The polymer of the ethylenically unsaturated monomer containing a hydrophilic group has a surface porous structure; The method for preparing the porous water-absorbing resin comprises the following steps: Step S1, weighing 45g of an ethylenically unsaturated monomer acrylic acid containing a hydrophilic group, adding 11.25g of water to dilute, under ice-water bath conditions, adding 83.3g of a 30% by mass NaOH solution dropwise to an aqueous solution of acrylic acid, stirring until the solution is transparent without precipitation, adding 0.0675g of an initiator potassium persulfate, 0.0112g of a cross-linking agent N,N-methylenebisacrylamide, and then adding 1.8g of a porogen sodium bicarbonate, mixing and stirring to obtain a solution to be polymerized; Step S2, adding 180 g of hydrocarbon dispersant n-heptane and 0.59 g of dispersant sucrose fatty acid ester into a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, stirring, heating to 70° C. until the sucrose fatty acid ester is completely dissolved, then adding the prepared solution to be polymerized, passing nitrogen, stirring at a speed of 350 r / min, and keeping warm at 70° C. for 1 to 2 h to initiate polymerization of sodium acrylate, and then heating to 80° C. and keeping warm for 1 h to complete the reaction of sodium acrylate to obtain a polymer suspension of ethylenically unsaturated monomers containing hydrophilic groups; Step S3, heating the polymer suspension of the ethylenically unsaturated monomer containing a hydrophilic group to 120° C. to separate water from the particles, and at the same time, accelerating the decomposition of sodium bicarbonate at high temperature to generate carbon dioxide, forming a porous structure inside the particles, and refluxing the solvent into the reactor. When the water content in the particles is reduced to less than 30%, the separation is terminated to obtain a dehydrated porous water-absorbing resin; Step S4, adding 1.2 g of ethylene glycol diglycidyl ether as a surface crosslinking agent, carrying out a surface crosslinking reaction at 80° C. for 1 h until the reaction is complete, cooling to room temperature, filtering, and collecting the filter cake as porous water-absorbing resin particles.

Citation Information

Patent Citations

  • Preparation method of super water absorbent resin

    CN102504288A

  • Preparation method of crylic acid resin with high water absorbability

    CN102516578A

  • Method for preparing super absorbent resin microspheres

    CN104448102A

  • Superabsorbent polymer having fast absorption

    CN104974312A

  • Poly-acrylic series water-absorbent resin, composition and manufacturing method of poly-acrylic series water-absorbent resin

    CN107722329A