A preparation method of Pd atomic cluster modified ZnO nanomaterial and its products and applications

ZnO nanofibers are prepared by electrospinning and Pd is modified inside the pores, which solves the problem of insufficient selectivity and stability of existing ZnO nanomaterials in hydrogen detection, achieves high sensitivity and specific detection, and improves hydrogen sensors. performance.

CN115748247BActive Publication Date: 2024-10-22SHANGHAI NAT ENG RES CENT FORNANOTECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211518497.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-10-22
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

Existing ZnO nanomaterials have problems with insufficient selectivity and long-term stability in hydrogen detection, making it difficult to achieve high sensitivity and specificity detection.

Method used

ZnO nanofibers were prepared by electrospinning, and hydrothermal reaction was carried out in a methanol solution of 2-methylimidazole to form a nanopore structure, and then Pd was modified inside the pores to improve the material's catalytic reaction ability for hydrogen.

Benefits of technology

Highly sensitive and specific detection of hydrogen is achieved, and the selectivity and stability of the gas sensor under long-term working conditions are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115748247B_ABST
    Figure CN115748247B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and product and application of a Pd atomic cluster modified ZnO nanomaterial, wherein Zn nanofibers are prepared by electrostatic spinning, and then hydrothermally reacted in a methanol solution of 2-methylimidazole to form a large number of nanometer-sized pores on the surface to achieve the screening of hydrogen, and the catalytic reaction of the material to hydrogen is improved by Pd modification inside the pores. The combined effect of the two factors can achieve highly sensitive and specific detection of hydrogen. The preparation method of the invention is simple, and the sensitivity and selectivity of ZnO nanomaterials to gas response are improved by increasing the material porosity and Pd doping, and the gas sensor is made into a gas sensor, which can increase the selectivity of the gas sensor to hydrogen and the stability under long-term working conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of gas detection, and in particular to a preparation method of a Pd atomic cluster modified ZnO nano material, a product and an application thereof. Background Art

[0002] Hydrogen is a toxic gas widely used in industry. It is colorless, flammable and explosive. With the rise of new energy, new energy materials based on hydrogen have shown broad application prospects. The resulting demand is for hydrogen detection in usage scenarios to prevent safety accidents caused by hydrogen leakage.

[0003] ZnO has become a gas-sensitive material for detecting a variety of toxic, harmful, flammable and explosive gases due to its good stability, easy synthesis and regulation of surface properties. However, pure semiconductor materials are not satisfactory in terms of selectivity and long-term stability. By constructing nanomaterials and doping, on the one hand, the specific surface area of ​​the material can be increased and the active sites of the surface reaction can be increased. On the other hand, doping can be used to enhance the catalytic reaction to specific gases.

[0004] The present invention adopts an electrospinning method to prepare a two-dimensional structured ZnO nanomaterial, grows ZIF-8 with an MOF structure on the surface of the nanomaterial, pyrolyzes the ZIF-8 organic framework during heat treatment, utilizes the pore size of the ZIF-8 to achieve selective adsorption of hydrogen, utilizes Pd modification to achieve a catalytic reaction at the adsorption site, and can prepare a gas sensor for hydrogen detection. Summary of the invention

[0005] The present invention aims to provide a method for preparing a Pd atomic cluster-modified ZnO nanomaterial.

[0006] Another object of the present invention is to provide a Pd atomic cluster modified ZnO nanomaterial product prepared by the above method.

[0007] Another object of the present invention is to provide an application of the above product.

[0008] The object of the present invention is achieved through the following scheme: a preparation method of a Pd atomic cluster modified ZnO nanomaterial, wherein Zn nanofibers are prepared by electrospinning, and then hydrothermally reacted in a methanol solution of 2-methylimidazole to form a large number of nanometer-sized pores on the surface to achieve hydrogen screening, and Pd modification inside the pores to enhance the catalytic reaction of the material to hydrogen. The combined effect of the two factors can achieve highly sensitive and specific detection of hydrogen, comprising the following steps:

[0009] Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.1-0.3 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers;

[0010] Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.6-0.8 M, take 0.3 g of the nanofibers obtained in step 1 and add them to the 2-methylimidazole methanol solution, stir for 30 min, place the resulting solution in a polytetrafluoroethylene reactor, and perform hydrothermal reaction at 180 °C for 24 h. After cooling to room temperature, centrifuge the sample, dry it at 80 °C, and grind it;

[0011] Step 3: Weigh 0.0012-0.0036 g of PdCl2 and dissolve it in 3-5 mL of deionized water to obtain an aqueous solution of PdCl2. Take 0.2 g of the sample ground in step 2 and add it to 10 mL of deionized water. After ultrasonic dispersion, drop the aqueous solution of PdCl2. After stirring for 30 min, freeze-dry the sample at -80 °C, grind the dried sample, and place it under an inert gas atmosphere for heat treatment.

[0012] Step 4: Take 0.004-0.01 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster-modified ZnO nanomaterials.

[0013] The inert gas atmosphere in step 3 is one of nitrogen or argon, the heat treatment temperature is 650-750°C, and the heating rate is 5-10°C / min.

[0014] The present invention also provides a Pd atomic cluster modified ZnO nanomaterial, which is prepared according to any of the above methods.

[0015] The present invention also provides a Pd atomic cluster modified ZnO nanomaterial, which is used in the high-sensitivity and specific detection of hydrogen and can be used as a gas sensor.

[0016] Zn nanofibers are prepared by electrospinning and then hydrothermally reacted in a methanol solution of 2-methylimidazole to form a large number of nano-sized pores on the surface to achieve hydrogen screening. The catalytic reaction of the material to hydrogen is enhanced by Pd modification inside the pores. The combined effect of these two factors can achieve highly sensitive and specific detection of hydrogen.

[0017] The preparation method of the present invention is simple, and the sensitivity and selectivity of ZnO nanomaterials to gas response are improved by increasing the material porosity and Pd doping, and the gas sensor is made into a gas sensing device, which can increase the selectivity of the gas sensor to hydrogen and the stability under long-term working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 : is the response-recovery curve of the gas sensor of the present invention to hydrogen with a concentration of 10 ppm at room temperature;

[0019] Figure 2 : is the response sensitivity of the gas sensor of the present invention to different gases at room temperature. DETAILED DESCRIPTION

[0020] Embodiment 1:

[0021] A Pd atomic cluster modified ZnO nanomaterial, wherein Zn nanofibers are prepared by electrospinning, and then hydrothermally reacted in a methanol solution of 2-methylimidazole to form a large number of nano-sized pores on the surface, is prepared according to the following steps:

[0022] Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone (K30) aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.1 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers;

[0023] Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.6 M, take 0.3 g of the Zn precursor nanofibers obtained in step 1 and add it to the 2-methylimidazole methanol solution. After stirring for 30 min, place the resulting solution in a polytetrafluoroethylene reactor and perform hydrothermal reaction at 180 °C for 24 h. After cooling to room temperature, centrifuge the sample, dry it at 80 °C, and grind it.

[0024] Step 3: Weigh 0.0012g of PdCl2 and dissolve it in 3-5mL deionized water to obtain an aqueous solution of PdCl2. Take 0.2g of the sample ground in step 2 and add it to 10mL deionized water. After ultrasonic dispersion, add the aqueous solution of PdCl2 dropwise. After stirring for 30 minutes, freeze-dry the sample at -80℃. Grind the freeze-dried sample and heat-treat it in an argon atmosphere at a temperature of 700℃ and a heating rate of 5℃ / min.

[0025] Step 4: Take 0.004 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster-modified ZnO nanomaterials.

[0026] Preparation of MEMS gas sensors based on Pd atomic clusters modified ZnO nanostructures:

[0027] Take the MEMS device with Pt interdigitated electrodes, ultrasonically clean it with deionized water and ethanol, blow it dry with a nitrogen gun, make the sample obtained in step 4 into a slurry, evenly apply it on the surface of the MEMS device, dry it, and place it in a muffle furnace for heat treatment at a temperature of 400 °C, a holding time of 1 h, and a heating rate of 2 °C / min. After the cavity cools to room temperature, take it out to obtain a MEMS gas sensor based on Pd atomic cluster-modified ZnO nanostructure.

[0028] Figure 1 This is the response-recovery curve of the gas sensor of the device obtained in this example to hydrogen with a concentration of 10 ppm at room temperature. The response sensitivity is 18.5, which shows that the gas sensor has very excellent response characteristics.

[0029] Embodiment 2:

[0030] A Pd atomic cluster modified ZnO nanomaterial is prepared in the following steps similar to those in Example 1:

[0031] Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone (K30) aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.3 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers;

[0032] Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.8 M, take 0.3 g of the nanofibers obtained in step 1 and add them to the 2-methylimidazole methanol solution. After stirring for 30 min, place the resulting solution in a polytetrafluoroethylene reactor and perform hydrothermal reaction at 180 °C for 24 h. After cooling to room temperature, centrifuge the sample, dry it at 80 °C, and grind it.

[0033] Step 3: Weigh 0.0024 g of PdCl2 and dissolve it in 3-5 mL of deionized water to obtain an aqueous solution of PdCl2. Take 0.2 g of the sample ground in step 2 and add it to 10 mL of deionized water. After ultrasonic dispersion, add the aqueous solution of PdCl2 dropwise. After stirring for 30 min, freeze-dry the sample at -80 °C. Grind the dried sample and heat-treat it in a nitrogen atmosphere at a temperature of 650 °C and a heating rate of 5 °C / min.

[0034] Step 4: Take 0.004 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster-modified ZnO nanomaterials.

[0035] Preparation of MEMS gas sensors based on Pd atomic clusters modified ZnO nanostructures:

[0036] Take the MEMS device with Pt interdigitated electrodes, ultrasonically clean it with deionized water and ethanol, blow it dry with a nitrogen gun, make the sample obtained in step 4 into a slurry, evenly apply it on the surface of the MEMS device, dry it, and place it in a muffle furnace for heat treatment at a temperature of 400 °C, a holding time of 1 h, and a heating rate of 2 °C / min. After the cavity cools to room temperature, take it out to obtain a MEMS gas sensor based on Pd atomic cluster-modified ZnO nanostructure.

[0037] The gas sensor of the device obtained in this example has a response-recovery curve to hydrogen with a concentration of 10 ppm at room temperature, and a response sensitivity of 21.4, indicating that the gas sensor has very excellent response characteristics.

[0038] Figure 2 The figure shows the response sensitivity of the device obtained in this embodiment to different gases.

[0039] Embodiment 3:

[0040] A Pd atomic cluster modified ZnO nanomaterial is prepared in the following steps similar to those in Example 1:

[0041] Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone (K30) aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.2 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers;

[0042] Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.7 M, take 0.3 g of the nanofibers obtained in step 1 and add them to the 2-methylimidazole methanol solution. After stirring for 30 min, place the resulting solution in a polytetrafluoroethylene reactor and perform hydrothermal reaction at 180 °C for 24 h. After cooling to room temperature, centrifuge the sample, dry it at 80 °C, and grind it.

[0043] Step 3: Weigh 0.0036 g of PdCl2 and dissolve it in 3-5 mL of deionized water to obtain an aqueous solution of PdCl2. Take 0.2 g of the sample ground in step 2 and add it to 10 mL of deionized water. After ultrasonic dispersion, add the aqueous solution of PdCl2 dropwise. After stirring for 30 min, freeze-dry the sample at -80 °C. Grind the dried sample and heat-treat it in an argon gas atmosphere at a temperature of 750 °C and a heating rate of 10 °C / min.

[0044] Step 4: Take 0.01 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster-modified ZnO nanomaterials.

[0045] Preparation of MEMS gas sensors based on Pd atomic clusters modified ZnO nanostructures:

[0046] Take the MEMS device with Pt interdigitated electrodes, ultrasonically clean it with deionized water and ethanol, blow it dry with a nitrogen gun, make the sample obtained in step 4 into a slurry, evenly apply it on the surface of the MEMS device, dry it, and place it in a muffle furnace for heat treatment at a temperature of 400 °C, a holding time of 1 h, and a heating rate of 2 °C / min. After the cavity cools to room temperature, take it out to obtain a MEMS gas sensor based on Pd atomic cluster-modified ZnO nanostructure.

[0047] The gas sensor of the device obtained in this example has a response-recovery curve to hydrogen with a concentration of 10 ppm at room temperature, and a response sensitivity of 18.9, indicating that the gas sensor has very excellent response characteristics.

Claims

1. A method for preparing a Pd atomic cluster modified ZnO nanomaterial, characterized in that: Zn nanofibers are prepared by electrospinning, and then hydrothermally reacted in a methanol solution of 2-methylimidazole to form a large number of nano-sized pores on the surface to achieve hydrogen screening. Pd is modified inside the pores to enhance the catalytic reaction of the material to hydrogen. The combined effect of the two factors enables highly sensitive and specific detection of hydrogen, including the following steps: Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.1-0.3 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers; Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.6-0.8 M, take 0.3 g of the Zn precursor nanofibers obtained in step 1 and add it to the 2-methylimidazole methanol solution. After stirring for 30 min, place the resulting solution in a polytetrafluoroethylene reactor, hydrothermally react at 180 ° C for 24 h, cool to room temperature, centrifuge the sample, dry it at 80 ° C, and grind it; Step 3: Weigh 0.0012-0.0036 g of PdCl2 and dissolve it in 3-5 mL of deionized water to obtain an aqueous solution of PdCl2. Take 0.2 g of the sample ground in step 2 and add it to 10 mL of deionized water. After ultrasonic dispersion, add the aqueous solution of PdCl2 dropwise. After stirring for 30 min, freeze-dry the sample at -80 °C. Grind the freeze-dried sample and place it for heat treatment under an inert gas atmosphere. Step 4: Take 0.004-0.01 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster modified ZnO nanomaterials; In step 3, the inert gas atmosphere is one of nitrogen or argon, the heat treatment temperature is 650-750°C, and the heating rate is 5-10°C / min.

2. The method for preparing a Pd atomic cluster modified ZnO nanomaterial according to claim 1, characterized in that: Prepare as follows: Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone K30 aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.1 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers; Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.6 M, take 0.3 g of the Zn precursor nanofibers obtained in step 1 and add it to the 2-methylimidazole methanol solution. After stirring for 30 min, place the resulting solution in a polytetrafluoroethylene reactor and perform hydrothermal reaction at 180 °C for 24 h. After cooling to room temperature, centrifuge the sample, dry it at 80 °C, and grind it. Step 3: Weigh 0.0012 g of PdCl2 and dissolve it in 3-5 mL of deionized water to obtain an aqueous solution of PdCl2. Take 0.2 g of the sample ground in step 2 and add it to 10 mL of deionized water. After ultrasonic dispersion, add the aqueous solution of PdCl2 dropwise. After stirring for 30 min, freeze-dry the sample at -80 °C. Grind the freeze-dried sample and heat-treat it in an argon atmosphere at a temperature of 700 °C and a heating rate of 5 °C / min. Step 4: Take 0.004 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster-modified ZnO nanomaterials.

3. The method for preparing a Pd atomic cluster modified ZnO nanomaterial according to claim 1, characterized in that: Prepare as follows: Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone K30 aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.3 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers; Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.8 M, take 0.3 g of the nanofibers obtained in step 1 and add them to the 2-methylimidazole methanol solution. After stirring for 30 min, place the resulting solution in a polytetrafluoroethylene reactor and perform hydrothermal reaction at 180 °C for 24 h. After cooling to room temperature, centrifuge the sample, dry it at 80 °C, and grind it. Step 3: Weigh 0.0024 g of PdCl2 and dissolve it in 3-5 mL of deionized water to obtain an aqueous solution of PdCl2. Take 0.2 g of the sample ground in step 2 and add it to 10 mL of deionized water. After ultrasonic dispersion, add the aqueous solution of PdCl2 dropwise. After stirring for 30 min, freeze-dry the sample at -80 °C. Grind the dried sample and heat-treat it in a nitrogen atmosphere at a temperature of 650 °C and a heating rate of 5 °C / min. Step 4: Take 0.004 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster-modified ZnO nanomaterials.

4. The method for preparing a Pd atomic cluster modified ZnO nanomaterial according to claim 1, characterized in that: Prepare as follows: Step 1: preparing zinc nitrate hexahydrate and polyvinyl pyrrolidone K30 aqueous solution in a mass ratio of 1:3, wherein the concentration of zinc salt is 0.2 mmol / mL, and after all of them are dissolved, electrospinning is performed at room temperature using an electrospinning device to prepare Zn precursor nanofibers; Step 2: Prepare 30 mL of 2-methylimidazole methanol solution at a molar concentration of 0.7 M, take 0.3 g of the nanofibers obtained in step 1 and add them to the 2-methylimidazole methanol solution. After stirring for 30 min, place the resulting solution in a polytetrafluoroethylene reactor and perform hydrothermal reaction at 180 °C for 24 h. After cooling to room temperature, centrifuge the sample, dry it at 80 °C, and grind it. Step 3: Weigh 0.0036 g of PdCl2 and dissolve it in 3-5 mL of deionized water to obtain an aqueous solution of PdCl2. Take 0.2 g of the sample ground in step 2 and add it to 10 mL of deionized water. After ultrasonic dispersion, add the aqueous solution of PdCl2 dropwise. After stirring for 30 min, freeze-dry the sample at -80 °C. Grind the dried sample and heat-treat it in an argon gas atmosphere at a temperature of 750 °C and a heating rate of 10 °C / min. Step 4: Take 0.01 g of ascorbic acid, dissolve it in 5 mL of deionized water, add the sample after heat treatment in step 3, ultrasonically disperse it for 10 min, centrifuge the sample, and obtain Pd atomic cluster-modified ZnO nanomaterials.

5. A Pd atomic cluster modified ZnO nanomaterial, characterized in that Prepared according to any one of claims 1 to 4.

6. Use of the Pd atomic cluster modified ZnO nanomaterial according to claim 5 in high-sensitivity and specific detection of hydrogen.

7. A method for preparing a gas sensor using the Pd atomic cluster modified ZnO nanomaterial according to claim 5, characterized in that: The MEMS device with Pt interdigital electrodes was taken, ultrasonically cleaned with deionized water and ethanol, and dried with a nitrogen gun. The Pd atomic clusters modified ZnO nanomaterials were made into a slurry and evenly coated on the surface of the MEMS device. After drying, it was placed in a muffle furnace for heat treatment at 400 °C, holding time of 1 h, and heating rate of 2 °C / min. After the cavity cooled to room temperature, it was taken out to obtain a MEMS gas sensor based on Pd atomic cluster modified ZnO nanostructure.

Citation Information

Patent Citations

  • Preparation method of metal or metal oxide particle-containing CeO2 fiber catalyst

    CN104707604A

  • Preparation method and application of ZnO-SnO2-Zn2SnO4 porous nanofiber gas sensitive material

    CN110865099A

  • Preparation method of Pd cluster modified ZnO / g-carbon nitride as well as product and application of Pd cluster modified ZnO / g-carbon nitride

    CN114130352A

  • Pd-ZnO nanocomposite based on ZIF-8 derivation and preparation method thereof, sensor and preparation method thereof

    CN115032240A