A ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes and preparation method thereof

Through the preparation of terpolymerized high-efficiency aldehyde-free color agent, textile solidification is solved by using raw materials such as dimethyldiallyl ammonium chloride and acyloxy cationic monomers, combined with multiple initiators to control the polymerization reaction, the textile solidification is solved The problem of insufficient wet friction and washing fastness of the toner has achieved efficient and environmentally friendly color fixation effect, and the fabric performance has been significantly improved and complied with green environmental standards.

CN115748271BActive Publication Date: 2024-11-15ZHEJIANG HAILIAN NEW MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211318513.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-26
Publication Date
2024-11-15
Estimated Expiration
2042-10-26

AI Technical Summary

Technical Problem

The existing textile color fixative has shortcomings in terms of wet friction fastness and washing color fastness, and the traditional process is complex and does not meet the green and environmental requirements. The dimethyldiallyl ammonium chloride color fixative has yellowing .

Method used

Using terpolymerized high-efficiency aldehyde-free colorant, consisting of dimethyldiallyl ammonium chloride, acyloxy-containing cationic monomer and crosslinking agent, the polymerization reaction is controlled through multiple initiator dropwise additions to form high-efficiency The cationic color fixing agent combines with anionic dye to form a complex, which improves the water washing fastness and dry and wet friction color fastness of the fabric.

Benefits of technology

It achieves a low-cost, efficient and environmentally friendly color fixation effect. The fabric has excellent washing fastness, stain fastness and dry and wet friction color fastness, and the process is simplified to meet the requirements of green and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003910422230000071
    Figure BDA0003910422230000071
Patent Text Reader

Abstract

The present invention provides a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes and a preparation method thereof, and belongs to the technical field of color fixing agents. The ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes is prepared from the following raw materials in parts by weight: 60 to 75 parts of dimethyldiallylammonium chloride solution, 1.0 to 7.0 parts of acyloxy cationic monomers, 5.0 to 12.0 parts of cross-linking agents, 0.1 to 0.5 parts of initiators, and 10 to 25 parts of deionized water. The ternary copolymer high-efficiency formaldehyde-free color fixing agent obtained by the present invention has low cost, high efficiency and environmental protection, and can better form complex color lakes with anionic dyes due to its strong cationicity. By introducing the active group acyloxy, it can react with the active group on the dye molecule and the active hydrogen on the cellulose molecule respectively, so that the dye is more closely combined with the fiber, so that the fabric after color fixing has excellent washing fastness, staining fastness and dry and wet friction color fastness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of color fixing agents, and in particular relates to a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes and a preparation method thereof. Background Art

[0002] The textile industry is a traditional industry in my country and plays a vital role in the development of the national economy. The color fixing agent is one of the indispensable and important auxiliaries in the printing and dyeing industry. In recent years, some developed countries have continuously improved the quality requirements of textile products in order to reverse the trade deficit. Among them, the most important are the requirements for color fastness of textiles and strict restrictions on free formaldehyde content.

[0003] CN103696296B discloses a cationic formaldehyde-free color fixing agent for active dyes and a preparation method thereof, which is mainly prepared from dimethyldiallylammonium chloride, a tertiary amino group-containing monomer and a crosslinking agent. By introducing active groups such as tertiary amino groups and ester groups to react with reactive groups on dye molecules and hydroxyl groups on cellulose molecules, the dye molecules are more firmly combined with fibers, thereby improving dry and wet friction fastness and washing color fastness. However, although the introduction of tertiary amino groups can improve the color fixing effect of the color fixing agent, the fabric will turn yellow after color fixing.

[0004] CN106811998B discloses a cross-linked formaldehyde-free color fixing agent emulsion and a preparation method thereof, which is mainly prepared by reverse emulsion polymerization process of dimethyldiallylammonium chloride monomer, diallylamine hydrochloride monomer, chelating agent, organic alkane solvent, emulsion stabilizer, emulsifier, oil-soluble thermal initiator and active activator, and the monomer is dispersed into fine bead particles by emulsification during the preparation process by adding organic alkane solvent. This method can obtain cross-linked formaldehyde-free color fixing agent emulsions with different cross-linking degrees and different molecular weights, but this method is not only complicated in process and high in cost, but also does not conform to the current concept of green environmental protection.

[0005] Dimethyldiallylammonium chloride is an ideal raw material for color fixing agents. It is non-toxic and pollution-free, meets the requirements of green environmental protection, and is cheaper than other quaternary ammonium salt cationic monomers. However, polydimethyldiallylammonium chloride color fixing agents have problems such as poor wet friction fastness and poor color fastness to washing. Summary of the invention

[0006] The present invention provides a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes and a preparation method thereof, so as to solve the above technical problems.

[0007] The invention provides a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes, which is prepared from the following raw materials in parts by weight: 60-75 parts of dimethyldiallylammonium chloride solution, 1.0-7.0 parts of acyloxy-containing cationic monomers, 5.0-12.0 parts of crosslinking agents, 0.1-0.5 parts of initiators, and 10-25 parts of deionized water.

[0008] Furthermore, the mass percentage concentration of the dimethyldiallylammonium chloride solution is 50-65%.

[0009] Furthermore, the acyloxy group-containing cationic monomer is at least one of methacryloyloxyethyl trimethyl ammonium chloride, acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl dimethyl benzyl ammonium chloride, and acryloyloxyethyl dimethyl benzyl ammonium chloride.

[0010] Furthermore, the cross-linking agent is at least one of diallylamine, triallylamine, and N-methyldiallylamine.

[0011] Furthermore, the initiator is at least one of the redox systems formed by sodium sulfite and ammonium persulfate, potassium persulfate, and sodium persulfate.

[0012] Furthermore, the negative charge requirement is 600-700ueq / L, the viscosity-average molecular weight is 100,000-300,000, the pH is 5-7, the sugar content is 58-62%, and the dynamic viscosity is 5000-15000mpa·s.

[0013] An embodiment of the present invention further provides a method for preparing any of the above-mentioned ternary copolymer high-efficiency formaldehyde-free color fixing agents for reactive dyes, comprising the following steps:

[0014] Mixing deionized water and an initiator to obtain an initiator solution;

[0015] Under nitrogen, add 1 / 5 to 1 / 4 of the total mass of dimethyldiallylammonium chloride solution into the reaction kettle, stir and heat to 70 to 80°C;

[0016] Start the first dropwise addition of the remaining dimethyldiallylammonium chloride solution;

[0017] At the same time, the second drop of acyloxy-containing cationic monomer and cross-linking agent is added;

[0018] At the same time, add 1 / 5 of the total amount of the initiator solution for the third time, and raise the temperature to 85-95°C after the addition is completed;

[0019] Fourth, add 2 / 5 of the total amount of the initiator solution, keep warm for 2-3 hours and then raise the temperature to 95-105°C;

[0020] Fifthly, 2 / 5 of the total amount of the initiator solution is added dropwise, and the temperature is kept for 2-3 hours, and the temperature is lowered to 40° C., and a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes is obtained.

[0021] Furthermore, the first dropping time is 1-3 hours; the second dropping time is 0.5-1 hour.

[0022] Furthermore, the third dropping time is 2-4 hours; the fourth dropping time is 1-2 hours; and the fifth dropping time is 1-2 hours.

[0023] The present invention has the following advantages:

[0024] The ternary copolymer high-efficiency formaldehyde-free color fixing agent proposed by the present invention has low cost, high efficiency and environmental protection. Because it has strong cationicity, it can better form complex color lakes with anionic dyes. By introducing active groups, acyloxy groups can react with active groups on dye molecules and active hydrogen on cellulose molecules, respectively, so that the dye and fiber are more closely combined, so that the fabric after color fixing has excellent washing fastness, staining fastness and dry and wet friction color fastness. In addition, by adding a small amount of cross-linking agent, the color fixing agent molecules after micro-cross-linking have better film-forming properties, further improving the color fixing effect of the color fixing agent. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. In the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other.

[0026] An embodiment of the present invention provides a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes, which is prepared from raw materials including the following parts by weight: 60 to 75 parts of dimethyldiallylammonium chloride solution, 1.0 to 7.0 parts of acyloxy cationic monomers, 5.0 to 12.0 parts of cross-linking agents, 0.1 to 0.5 parts of initiators, and 10 to 25 parts of deionized water.

[0027] The ternary copolymer high-efficiency formaldehyde-free color fixing agent for active dyes proposed in the embodiment of the present invention has strong cationicity and can better form complex lakes with anionic dyes; by introducing active groups acyloxy groups, they can react with active groups on dye molecules and active hydrogen on cellulose molecules, respectively, so that the dye and fiber are more closely combined, so that the fabric after color fixing has excellent washing fastness, staining fastness and dry and wet friction color fastness. In addition, by adding a small amount of crosslinking agent, the film-forming property of the color fixing agent molecules after micro-crosslinking is better, further improving the color fixing effect of the color fixing agent.

[0028] In one embodiment of the present invention, the mass percentage concentration of the dimethyldiallylammonium chloride solution is 50-65%. Preferably, the mass percentage concentration of the dimethyldiallylammonium chloride solution is 60%.

[0029] In one embodiment of the present invention, the acyloxy group-containing cationic monomer is at least one of methacryloyloxyethyl trimethyl ammonium chloride, acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl dimethyl benzyl ammonium chloride, and acryloyloxyethyl dimethyl benzyl ammonium chloride. Preferably, the acyloxy group-containing cationic monomer is methacryloyloxyethyl trimethyl ammonium chloride.

[0030] In one embodiment of the present invention, the cross-linking agent is at least one of diallylamine, triallylamine, and N-methyldiallylamine. Preferably, the cross-linking agent is diallylamine.

[0031] In one embodiment of the present invention, the initiator is at least one of the redox systems formed by sodium sulfite and ammonium persulfate, potassium persulfate, and sodium persulfate. Preferably, the initiator is a sodium sulfite-ammonium persulfate redox system.

[0032] Wherein, the molar ratio of sodium sulfite to ammonium persulfate, potassium persulfate or sodium persulfate is 1:1.

[0033] In one embodiment of the present invention, the negative charge requirement of the obtained ternary copolymer high-efficiency formaldehyde-free fixing agent for reactive dyes is 600-700ueq / L, the viscosity-average molecular weight is 100,000-300,000, the pH is 5-7, the sugar content is 58-62%, and the dynamic viscosity is 5000-15000mpa·s.

[0034] An embodiment of the present invention further provides a method for preparing the ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes as described in any one of the above items, comprising the following steps:

[0035] Mixing deionized water and an initiator to obtain an initiator solution;

[0036] Under nitrogen, add 1 / 5 to 1 / 4 of the total mass of dimethyldiallylammonium chloride solution into the reaction kettle, stir and heat to 70 to 80°C;

[0037] Start the first dropwise addition of the remaining dimethyldiallylammonium chloride solution;

[0038] At the same time, the second drop of acyloxy-containing cationic monomer and cross-linking agent is added;

[0039] At the same time, add 1 / 5 of the total amount of the initiator solution for the third time, and raise the temperature to 85-95°C after the addition is completed;

[0040] Fourth, add 2 / 5 of the total amount of the initiator solution, keep warm for 2-3 hours and then raise the temperature to 95-105°C;

[0041] Fifthly, 2 / 5 of the total amount of the initiator solution is added dropwise, and the temperature is kept for 2-3 hours, and the temperature is lowered to 40° C., and a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes is obtained.

[0042] The ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes provided in the embodiment of the present invention can make the polymerization reaction more complete by adding the initiator in multiple times, which is beneficial to improving the monomer conversion rate and further enhancing the color fixing effect.

[0043] In one embodiment of the present invention, the first dropping time is 1-3 hours; the second dropping time is 0.5-1 hour.

[0044] In one embodiment of the present invention, the third dropping time is 2-4 hours; the fourth dropping time is 1-2 hours; and the fifth dropping time is 1-2 hours.

[0045] The application of the ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes proposed in the embodiment of the present invention can be used for color fixing of various fabrics dyed with reactive dyes in the textile industry. The fixed fabrics have excellent washing fastness, staining fastness and dry and wet rubbing color fastness.

[0046] The present invention will be described in detail below with reference to embodiments.

[0047] The entire reaction process is carried out in a stainless steel atmospheric pressure reactor which is replaced with nitrogen and equipped with a stirrer and can control the temperature. In the embodiments and comparative examples, all materials are measured by mass fraction.

[0048] Example 1 A method for preparing a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes comprises the following steps:

[0049] Mix 13.4 parts of deionized water and 0.5 parts of an initiator (sodium sulfite and ammonium persulfate in a molar ratio of 1:1) to obtain an initiator solution;

[0050] Under nitrogen, add 75 parts of 60% dimethyldiallylammonium chloride solution (1 / 5 of the total mass) into the reaction kettle, stir and heat to 75°C;

[0051] Start the first dropwise addition (time 1.5 h) of the remaining dimethyldiallylammonium chloride solution;

[0052] At the same time, 6 parts of acyloxy-containing cationic monomer (methacryloyloxyethyl dimethylbenzyl ammonium chloride) and 8 parts of crosslinking agent (diallylamine) were added dropwise for the second time (time 0.7 h);

[0053] At the same time, add 1 / 5 of the total amount of the initiator solution for the third time (time: 3h), and after the addition is completed, heat it to 90°C;

[0054] Fourthly, add dropwise (time: 1.5h) 2 / 5 of the total amount of the initiator solution, keep warm for 2-3h and then raise the temperature to 100°C;

[0055] Fifthly, add dropwise (time is 1.5h) 2 / 5 of the total amount of the initiator solution, keep warm for 2-3h, cool down to 40°C, and obtain a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes.

[0056] The performance of the obtained ternary copolymer high-efficiency formaldehyde-free fixing agent for reactive dyes was measured according to the national standard detection method, and the final results were: charge demand was 613μeq / L, viscosity average molecular weight was 152,300, sugar content was 60.0%, and dynamic viscosity was 5143mpa·s.

[0057] Example 2 A method for preparing a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes comprises the following steps:

[0058] Mix 20 parts of deionized water and 0.2 parts of initiator (sodium sulfite and potassium persulfate in a molar ratio of 1:1) to obtain an initiator solution;

[0059] Under nitrogen, add 72.5 parts of 60% dimethyldiallylammonium chloride solution (1 / 4 of the total mass) into the reaction kettle, stir and heat to 80°C;

[0060] Start the first dropwise addition (time is 3 h) of the remaining dimethyldiallylammonium chloride solution;

[0061] At the same time, 5 parts of acyloxy-containing cationic monomer (methacryloyloxyethyl trimethylammonium chloride) and 10 parts of crosslinking agent (triallylamine) were added dropwise for a second time (time of 1 hour);

[0062] At the same time, add 1 / 5 of the total amount of the initiator solution for the third time (4h), and heat to 95℃ after the addition is completed;

[0063] Fourthly, add dropwise (time: 2h) 2 / 5 of the total amount of the initiator solution, keep warm for 2-3h and then raise the temperature to 105°C;

[0064] Fifthly, add dropwise (time is 2h) 2 / 5 of the total amount of the initiator solution, keep warm for 2-3h, cool down to 40°C, and obtain a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes.

[0065] The performance of the obtained ternary copolymer high-efficiency formaldehyde-free fixing agent for reactive dyes was measured according to the national standard detection method, and the final results were: charge demand of 627 μeq / L, viscosity average molecular weight of 163,100, sugar content of 60.8%, and dynamic viscosity of 11851 mpa·s.

[0066] Example 3

[0067] A method for preparing a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes comprises the following steps:

[0068] An initiator solution was prepared by mixing 16 parts of deionized water and 0.4 parts of an initiator (sodium sulfite and sodium persulfate in a molar ratio of 1:1);

[0069] Under nitrogen, add 73 parts of 62% dimethyldiallylammonium chloride solution (1 / 5 of the total mass) into the reaction kettle, stir and heat to 70°C;

[0070] Start the first dropwise addition (time 12h) of the remaining dimethyldiallylammonium chloride solution;

[0071] At the same time, 4 parts of acyloxy-containing cationic monomer (acryloyloxyethyl trimethyl ammonium chloride) and 10 parts of crosslinking agent (N-methyldiallylamine) were added dropwise for the second time (time 0.6 h);

[0072] At the same time, add 1 / 5 of the total amount of the initiator solution for the third time (time is 2h), and after the addition is completed, heat it to 85°C;

[0073] Fourthly, add dropwise (time: 1h) 2 / 5 of the total amount of the initiator solution, keep warm for 2-3h and then raise the temperature to 95°C;

[0074] Fifthly, add dropwise (time is 1 hour) 2 / 5 of the total amount of the initiator solution, keep warm for 2-3 hours, cool down to 40°C, and obtain a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes.

[0075] The performance of the obtained ternary copolymer high-efficiency formaldehyde-free fixing agent for reactive dyes was measured according to the national standard detection method, and the final results were: charge demand of 623 μeq / L, viscosity average molecular weight of 208,500, sugar content of 59%, and dynamic viscosity of 9027 mpa·s.

[0076] Comparative Example 1

[0077] Same as Example 1, except that no acyloxy-containing cationic monomer is added.

[0078] The properties of the obtained formaldehyde-free color fixing agent were measured according to the national standard testing method, and the final results were: charge demand of 525 μeq / L, viscosity average molecular weight of 153,200, sugar content of 61.3%, and dynamic viscosity of 10235 mpa·s.

[0079] Comparative Example 2

[0080] The same as Example 1, except that, under nitrogen, all the dimethyldiallylammonium chloride solution was added to the reaction kettle, and then stirred and heated; and all the initiator solution was added dropwise during the third addition.

[0081] The properties of the obtained formaldehyde-free color fixing agent were measured according to the national standard testing method, and the final results were: the charge demand was 554 μeq / L, the viscosity-average molecular weight was 132,700, the sugar content was 61.1%, and the dynamic viscosity was 9736 mpa·s.

[0082] Test Example 1

[0083] The cotton fabric dyed with reactive scarlet CMC Rea.Red 194 was treated with the high-efficiency formaldehyde-free fixing agent prepared in Examples 1 to 3 and Comparative Examples 1 to 2, using an immersion fixing process with a fixing agent dosage of 1% (owf), a pH of 5 to 7, a bath ratio of 1:10, a temperature of 40°C, and a time of 30 min.

[0084] The performance of the cotton fabric after color fixation was tested according to the national standard testing method. The main performance indicators are shown in Table 1.

[0085] Table 1

[0086]

[0087] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes, characterized in that: The steps include: Mixing deionized water and an initiator to obtain an initiator solution; Under nitrogen, add 1 / 5 to 1 / 4 of the total mass of dimethyldiallylammonium chloride solution into the reaction kettle, stir and heat to 70 to 80°C; Start the first dropwise addition of the remaining dimethyldiallylammonium chloride solution; At the same time, the second drop of acyloxy-containing cationic monomer and cross-linking agent is added; At the same time, add 1 / 5 of the total amount of the initiator solution for the third time, and raise the temperature to 85-95°C after the addition is completed; Fourth, add 2 / 5 of the total amount of the initiator solution, keep warm for 2-3 hours and then raise the temperature to 95-105°C; Fifth, add 2 / 5 of the total amount of the initiator solution, keep warm for 2-3 hours, cool down to 40°C, and obtain a ternary copolymer high-efficiency formaldehyde-free color fixing agent for reactive dyes; The reactive dye ternary copolymer high-efficiency formaldehyde-free color fixing agent is prepared from the following raw materials in parts by weight: 60-75 parts of dimethyldiallylammonium chloride solution, 1.0-7.0 parts of acyloxy-containing cationic monomers, 5.0-12.0 parts of crosslinking agents, 0.1-0.5 parts of initiators, and 10-25 parts of deionized water; The acyloxy-containing cationic monomer is at least one of methacryloyloxyethyl trimethyl ammonium chloride, acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl dimethyl benzyl ammonium chloride, and acryloyloxyethyl dimethyl benzyl ammonium chloride; The cross-linking agent is at least one of diallylamine, triallylamine, and N-methyldiallylamine; The initiator is at least one of the redox systems formed by sodium sulfite and ammonium persulfate, potassium persulfate, and sodium persulfate.

2. The preparation method according to claim 1, characterized in that: The mass percentage concentration of the dimethyldiallylammonium chloride solution is 50-65%.

3. The preparation method according to claim 1, characterized in that: The negative charge requirement is 600-700ueq / L, the viscosity-average molecular weight is 100,000-300,000, the pH is 5-7, the sugar content is 58-62%, and the dynamic viscosity is 5000-15000mpa·s.

4. The preparation method according to claim 1, characterized in that: The first dropwise addition time is 1-3 hours; the second dropwise addition time is 0.5-1 hour.

5. The preparation method according to claim 1, characterized in that: The third dropping time is 2-4 hours; the fourth dropping time is 1-2 hours; and the fifth dropping time is 1-2 hours.