Used to reduce SO in flue gas x with NO x Catalyst, preparation method and application, flue gas SO removal x and NO x Methods
By preparing catalysts containing rare earth and non-noble metal components, the problems of high cost and inability to simultaneously remove SOx and NOx in the existing technology are solved, and efficient and economical flue gas purification effects are achieved.
Patent Information
- Application Number
- CN202111055118.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-09-09
AI Technical Summary
The existing technology is costly to reduce the emissions of SOx and NOx in catalytic cracking regeneration flue gas and cannot remove both at the same time. The amount of additives is too large, which affects the economy.
A catalyst is used, which consists of 25-95% inorganic oxide matrix, 2-70% rare earth metal components, 1-30% IIA group metal components, 1-15% VB, VIII, IB , Group IIB non-noble metal components, It consists of 1-10% non-noble metal components of Group VIIB and 0.01-1.5% precious metal components. It is prepared by co-precipitation method or sol-gel method. Combined with the introduction of precious metals, it improves the redox capacity of the catalyst and promotes SOx oxidation and NOx reduction. .
It effectively reduces the emissions of SOx and NOx in the catalytic cracking regeneration flue gas, reduces the amount of precious metals, reduces the cost, and at the same time improves the removal efficiency of the catalyst, achieving the purpose of removing SOx and NOx at the same time.
Smart Images

Figure BDA0003254298650000211 
Figure BDA0003254298650000221 
Figure BDA0003254298650000222
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of industrial catalysis, and in particular to a method for simultaneously reducing SO x with NO x Catalyst and preparation method and application thereof, and a flue gas simultaneous SO removal x and NO x method. Background Art
[0002] During the catalytic cracking reaction, the reaction of hydrocarbons causes coke to deposit on the catalyst, which reduces the activity of the catalyst. The catalyst containing coke is sent to the regenerator after the hydrocarbons adsorbed on the catalyst are removed by the stripping section. In the regenerator, the catalyst containing coke is fully exposed to air at high temperature, and the coke on the catalyst surface is burned off, so that the activity of the catalyst can be restored. SO2 is generated when the catalyst is burned. x and NO x These gases are discharged into the air and cause atmospheric pollution. As environmental protection requirements become more and more stringent, the emission standards for flue gas pollutants are becoming more and more stringent.
[0003] At present, the main technical measures to reduce the emission of catalytic cracking regeneration flue gas pollutants include: regenerator optimization, the use of additives and flue gas post-treatment. Among them, the method of adding additives is widely used because of its advantages such as flexible operation and no investment in facilities. At present, desulfurization and denitrification additives are mainly used to remove a flue gas pollutant alone. For example: CN1334316A discloses a composition containing magnesium aluminum spinel and a sulfur transfer agent of cerium / vanadium oxide, which is used to remove SO from catalytic cracking flue gas. x CN101311248B provides a method for reducing NO in catalytic cracking regeneration flue gas. x Composition for reducing NO in catalytic cracking flue gas x .
[0004] The above patent document separately removes SO from the regeneration flue gas. x and NO x It has a good removal effect, but it cannot remove nitrogen oxides and sulfur oxides at the same time. In addition, the total amount of additives added is too large, and the cost is high. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem of high cost of existing desulfurization and denitrification technologies and to provide a method for simultaneously reducing SO x with NO x Catalyst and preparation method and application thereof, and a flue gas simultaneous SO removal x and NO x The catalyst preparation method provided by the present invention is simple and can effectively reduce SO in flue gas.x and NO x emissions.
[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for simultaneously reducing SO in flue gas. x with NO x The catalyst contains, based on the total weight of the catalyst, 25-95% by weight of an inorganic oxide matrix; 2-70% by weight of a rare earth metal component calculated as oxide; 1-30% by weight of a Group IIA metal component calculated as oxide; 1-15% by weight of one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB calculated as oxide; 1-10% by weight of a Group VIIB non-precious metal component calculated as oxide; and 0.01-1.5% by weight of a precious metal component calculated as an element.
[0007] Preferably, calculated as metal elements, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from VB, VIII, IB, and IIB groups is (0.4-18):1, more preferably (0.5-12):1, and even more preferably (1-6):1.
[0008] The second aspect of the present invention provides a method for simultaneously reducing SO in flue gas. x with NO x A method for preparing a catalyst, the method comprising the following steps:
[0009] (1) obtaining active metal precursors by coprecipitation or sol-gel method;
[0010] (2) mixing and slurrying the active metal precursor with the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and optionally the precious metal component precursor to obtain a slurry, and drying and / or calcining the slurry to obtain a composition;
[0011] The method may further optionally include: (3) impregnating the composition obtained in step (2) with a solution containing a noble metal component precursor as an impregnation solution to obtain a solid product, and then drying and / or calcining the solid product;
[0012] The active metal in the active metal precursor includes a rare earth metal component, a Group IIA metal component, one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB, and a Group VIIB non-precious metal component;
[0013] The active metal precursor, inorganic oxide matrix and / or inorganic oxide matrix precursor and precious metal component precursor are used in such amounts that the prepared catalyst contains, based on the total weight of the catalyst, 25-95 wt % of inorganic oxide matrix; 2-70 wt % of rare earth metal components calculated as oxides; 1-30 wt % of Group IIA metal components calculated as oxides; 1-15 wt % of one or more non-precious metal components selected from Groups VB, VIII, IB and IIB calculated as oxides; 1-10 wt % of Group VIIB non-precious metal components calculated as oxides; and 0.01-1.5 wt % of precious metal components calculated as elements.
[0014] The third aspect of the present invention provides a catalyst according to the first aspect and a catalyst prepared by the preparation method according to the second aspect for simultaneously removing SO from catalytic cracking regeneration flue gas. x and NO x Application in reaction.
[0015] A fourth aspect of the present invention provides a method for simultaneously removing SO from flue gas. x and NO x The method comprises: removing SO x and NO x Under the conditions of SO x and NO x The flue gas is contacted with the catalyst described in the first aspect and the catalyst prepared by the preparation method described in the second aspect.
[0016] The catalyst provided by the present invention can effectively reduce NO in catalytic cracking regeneration flue gas x and SO x The reason for this may be that the introduction of trace precious metals changes the geometric electronic structure of other metal oxide compositions in the catalyst, greatly improving its redox ability, which is beneficial to promoting SO x Oxidation and NO x On this basis, the combination of one or more non-precious metal components of VB, VIII, IB, and IIB groups and IIA group metal components can greatly improve the removal of NO by the catalyst combination. x and SO x The catalyst preparation method provided by the present invention is simple and can effectively reduce SO in catalytic cracking regeneration flue gas. x and NO x During this process, NO is adsorbed and dissociated by the catalyst. x Can promote SO x Converted into sulfate, thereby achieving simultaneous removal of SO x and NO x purpose. DETAILED DESCRIPTION
[0017] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0018] The first aspect of the present invention provides a method for simultaneously reducing SO in flue gas. x with NO x The catalyst is characterized in that, based on the total weight of the catalyst, it contains 25-95% by weight of an inorganic oxide matrix; 2-70% by weight of a rare earth metal component calculated as oxide; 1-30% by weight of a Group IIA metal component calculated as oxide; 1-15% by weight of one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB calculated as oxide; 1-10% by weight of a Group VIIB non-precious metal component calculated as oxide; and 0.01-1.5% by weight of a precious metal component calculated as an element.
[0019] According to the present invention, preferably, based on the total weight of the catalyst, it contains 40-90 wt% of an inorganic oxide matrix; 4-50 wt% of a rare earth metal component in terms of oxide; 1-20 wt% of a Group IIA metal component in terms of oxide; 2-12 wt% of one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB in terms of oxide; 1-8 wt% of a Group VIIB non-precious metal component in terms of oxide; 0.02-1.2 wt% of a precious metal component in terms of element; more preferably, based on the total weight of the catalyst, it contains 50-80 wt% of an inorganic oxide matrix; 4-40 wt% of a rare earth metal component in terms of oxide; 2-15 wt% of a Group IIA metal component in terms of oxide; 2-10 wt% of one or more non-precious metal components selected from VB, VIII, IB, IIB groups in terms of materials; 2-5 wt% of VIIB group non-precious metal components in terms of oxides; 0.02-1.0 wt% of precious metal components in terms of elements; most preferably, based on the total weight of the catalyst, it contains 50-80 wt% of inorganic oxide matrix; 7-38 wt% of rare earth metal components in terms of oxides; 2-8 wt% of IIA group metal components in terms of oxides; 2-7 wt% of one or more non-precious metal components selected from VB, VIII, IB, IIB groups in terms of oxides; 2-5 wt% of VIIB group non-precious metal components in terms of oxides; 0.02-0.05 wt% of precious metal components in terms of elements. Under the above preferred embodiment, the use of the above metals in specific contents can greatly reduce the amount of precious metals used and reduce costs.
[0020] According to the present invention, conventionally defined rare earth metal components can be used in the present invention. In order to further improve the removal of SO x with NO x The rare earth metal component is preferably selected from one or more of lanthanum, cerium, praseodymium and neodymium, more preferably lanthanum and / or cerium, most preferably lanthanum.
[0021] According to the present invention, the Group IIA metal component is selected from one or more of beryllium, magnesium, calcium, strontium and barium, and more preferably magnesium.
[0022] The VB group non-precious metal component may be selected from at least one of vanadium, niobium and tantalum; the VIII group non-precious metal component may be selected from at least one of iron, cobalt and nickel; the IB group non-precious metal component may be copper; the IIB group non-precious metal component may be selected from at least one of zinc, cadmium and mercury.
[0023] Preferably, the one or more non-precious metal components of groups VB, VIII, IB, and IIB are selected from one or more of iron, cobalt, nickel, copper, zinc, and vanadium, more preferably cobalt and / or iron, most preferably cobalt.
[0024] Preferably, the Group VIIB non-noble metal component is manganese.
[0025] Preferably, the noble metal component is selected from one or more of ruthenium, rhodium, rhenium, platinum, palladium, silver, iridium and gold, more preferably one or more of platinum, palladium and rhodium, most preferably palladium.
[0026] According to the catalyst provided by the present invention, the inorganic oxide matrix can be various inorganic oxide matrices conventionally used in the art, for example, at least one selected from alumina, silica-alumina, zeolite, spinel, kaolin, diatomaceous earth, perlite and perovskite. In the present invention, the spinel can be various commonly used spinels, for example, it can be at least one of magnesium aluminum spinel, zinc aluminum spinel and titanium aluminum spinel.
[0027] According to a preferred embodiment of the present invention, the inorganic oxide matrix is aluminum oxide.
[0028] In the present invention, the alumina may be at least one selected from γ-alumina, δ-alumina, η-alumina, ρ-alumina, κ-alumina and χ-alumina, and the present invention has no particular limitation on this.
[0029] According to a preferred embodiment of the present invention, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from VB, VIII, IB, and IIB groups, calculated as metal elements, is (0.4-18):1, further preferably (0.5-12):1, and further preferably (1-6):1.
[0030] According to a particularly preferred embodiment of the present invention, based on the total weight of the catalyst, it contains 50-80 wt% of aluminum oxide; 7-38 wt% of lanthanum in oxide form; 2-8 wt% of magnesium in oxide form; 2-7 wt% of cobalt in oxide form; 2-5 wt% of manganese in oxide form; 0.02-0.05 wt% of palladium in element form; more preferably, the molar ratio of lanthanum to cobalt is (1-6):1. The inventors of the present invention have found in the course of research that the use of rare earth element La, IIA group element Mg and transition non-precious metal elements containing Co and Mn in combination with at least one of the precious metal elements as active components can effectively reduce the NO in catalytic cracking regeneration flue gas. x and SO xThe reason may be that the introduction of trace precious metals changes the geometric electronic structure of the metal oxide composition, greatly improving its redox ability, which is conducive to promoting SO x Oxidation and NO x On this basis, the reduction of NO x Mn has good decomposition ability and SO x Mg, with its good adsorption capacity, significantly improves the removal of NO by the catalyst combination x and SO x ability.
[0031] The second aspect of the present invention provides a method for simultaneously reducing SO in flue gas. x with NO x A method for preparing a catalyst, the method comprising the following steps:
[0032] (1) obtaining active metal precursors by coprecipitation or sol-gel method;
[0033] (2) mixing and slurrying the active metal precursor with the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and optionally the precious metal component precursor to obtain a slurry, and drying and / or calcining the slurry to obtain a composition;
[0034] The method may further optionally include: (3) impregnating the composition obtained in step (2) with a solution containing a noble metal component precursor as an impregnation solution to obtain a solid product, and then drying and / or calcining the solid product;
[0035] The active metal in the active metal precursor includes a rare earth metal component, a Group IIA metal component, one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB, and a Group VIIB non-precious metal component;
[0036] The active metal precursor, inorganic oxide matrix and / or inorganic oxide matrix precursor and precious metal component precursor are used in such amounts that the prepared catalyst contains, based on the total weight of the catalyst, 25-95 wt % of inorganic oxide matrix; 2-70 wt % of rare earth metal components calculated as oxides; 1-30 wt % of Group IIA metal components calculated as oxides; 1-15 wt % of one or more non-precious metal components selected from Groups VB, VIII, IB and IIB calculated as oxides; 1-10 wt % of Group VIIB non-precious metal components calculated as oxides; and 0.01-1.5 wt % of precious metal components calculated as elements.
[0037] According to the present invention, preferably, the active metal precursor, the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and the noble metal component precursor are used in such an amount that the prepared catalyst contains, based on the total weight of the catalyst, 40-90 wt % of the inorganic oxide matrix; 4-50 wt % of the rare earth metal component in terms of oxide; 1-20 wt % of the IIA group metal component in terms of oxide; 2-12 wt % of one or more non-noble metal components selected from VB, VIII, IB, and IIB groups in terms of oxide; 1-8 wt % of the VIIB group non-noble metal component in terms of oxide; and 0.02-1.2 wt % of the noble metal component in terms of element. More preferably, the active metal precursor, the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and the noble metal component precursor are used in such an amount that the prepared catalyst contains, based on the total weight of the catalyst, 5-80 wt % of the inorganic oxide matrix; oxide matrix; 4-40 wt. % rare earth metal components calculated as oxides; 2-15 wt. % Group IIA metal components calculated as oxides; 2-10 wt. % non-precious metal components selected from VB, VIII, IB, and IIB groups calculated as oxides; 2-5 wt. % Group VIIB non-precious metal components calculated as oxides; 0.02-1.0 wt. % precious metal components calculated as elements; most preferably, based on the total weight of the catalyst, it contains 50-80 wt. % of an inorganic oxide matrix; 7-38 wt. % rare earth metal components calculated as oxides; 2-8 wt. % Group IIA metal components calculated as oxides; 2-7 wt. % non-precious metal components selected from VB, VIII, IB, and IIB groups calculated as oxides; 2-5 wt. % Group VIIB non-precious metal components calculated as oxides; 0.02-0.05 wt. % precious metal components calculated as elements.
[0038] Preferably, in the active component precursor, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from groups VB, VIII, IB, and IIB, calculated as metal elements, is (0.4-18):1, further preferably (0.5-12):1, and even more preferably (1-6):1.
[0039] In the method provided by the present invention, the selection range of the specific types of the rare earth metal component, the IIA group metal component, the one or more non-precious metal components of the VB, VIII, IB, and IIB groups, the VIIB group non-precious metal component, and the precious metal component and the inorganic oxide matrix are as described in the first aspect above and will not be repeated here.
[0040] The method provided by the present invention can be a coprecipitation method or a sol-gel method, and the coprecipitation method is more preferred. Preferably, step (1) adopts the coprecipitation method to obtain the active metal precursor; more preferably, the coprecipitation method comprises:
[0041] (1-1) providing a first solution containing a rare earth metal component precursor, a Group IIA metal component precursor, one or more non-noble metal component precursors selected from Groups VB, VIII, IB, and IIB, and a Group VIIB non-noble metal component precursor;
[0042] (1-2) subjecting the first solution to a coprecipitation reaction with a coprecipitant;
[0043] (1-3) Drying and / or calcining the solid product obtained by the coprecipitation reaction.
[0044] The present invention has no particular limitation on the method for obtaining the first solution in step (1-1), as long as the metal component precursors are mixed evenly. For example, the metal component precursors can be dissolved in water and stirred evenly.
[0045] According to the present invention, preferably, the rare earth metal component precursor, the IIA group metal component precursor, one or more non-precious metal component precursors selected from the VB, VIII, IB, IIB groups, and the VIIB group non-precious metal component precursor can be independently selected from the water-soluble salts of each metal component, such as nitrates, chlorides, chlorates or sulfates, etc., preferably nitrates and / or chlorides. In particular, the manganese precursor can be potassium permanganate and / or manganese chloride.
[0046] According to the present invention, the precious metal component precursor can be selected from any water-soluble compound containing the precious metal component. Preferably, the precious metal component precursor is selected from at least one of palladium nitrate, palladium chloride, chloroplatinic acid and rhodium chloride, and is further preferably palladium nitrate and / or palladium chloride.
[0047] The present invention has no particular limitation on the type and amount of the coprecipitant, as long as the coprecipitation reaction can proceed smoothly. The type of the coprecipitant can be a conventional choice in the art, preferably, the coprecipitant is a carbonate, further preferably at least one selected from ammonium carbonate, potassium carbonate and sodium carbonate, more preferably ammonium carbonate.
[0048] In step (1-2), the coprecipitant can be introduced in the form of a solution to undergo a coprecipitation reaction with the first solution. The present invention has no particular limitation on the concentrations of the first solution and the coprecipitant solution, as long as the solution concentration is less than the solubility during preparation, thereby ensuring that the coprecipitation reaction can fully occur.
[0049] Preferably, the coprecipitation reaction is carried out at a pH of 8-10, preferably 8.5-9.5. The pH of the coprecipitation reaction can be adjusted by adding acid and / or base, and there is no particular limitation on the specific type thereof, for example, it can be ammonia water.
[0050] According to the present invention, the process further comprises subjecting the reaction product obtained by the coprecipitation reaction to solid-liquid separation (for example, filtration or centrifugal separation) to obtain the solid product.
[0051] Preferably, the drying conditions in step (1-3) include: temperature of 60-150° C. and time of 4-12 h.
[0052] Preferably, the calcination conditions in step (1-3) include: temperature of 300-800° C. and time of 1-8 h.
[0053] The precious metal component of the present invention can be introduced in step (2) or in step (3), or partially in step (2) and partially in step (3). It is preferably introduced in step (3). This preferred embodiment is more conducive to the dispersion of the precious metal.
[0054] The precursor of the inorganic oxide matrix is any substance that can be converted into an oxide matrix by subsequent calcination. Those skilled in the art can make appropriate selections based on the specific types of the specific inorganic oxide matrix, and the present invention will not go into details here. For example, the precursor of aluminum oxide can be selected from various sols or gels of aluminum, or aluminum hydroxide. The aluminum hydroxide can be selected from at least one of gibbsite, diaspore, gibbsite, boehmite, and pseudo-boehmite. The most preferred precursor of aluminum oxide is pseudo-boehmite.
[0055] According to the preparation method provided by the present invention, the inorganic oxide matrix is aluminum oxide. Preferably, before slurrying, the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix is subjected to an acidification treatment. The acidification treatment can be carried out according to conventional technical means in the art. Further preferably, the acid used in the acidification treatment is hydrochloric acid.
[0056] The present invention has a wide range of selection of conditions for the acidification treatment. Preferably, the conditions for the acidification treatment include: an acid-aluminum ratio of 0.12-0.22:1, and a time of 20-40 min.
[0057] In the present invention, unless otherwise specified, the acid-to-aluminum ratio refers to the mass ratio of hydrochloric acid calculated as 36 wt % concentrated hydrochloric acid to the alumina precursor calculated on a dry basis.
[0058] The specific implementation of the acidification peptization treatment may be: adding the aluminum oxide precursor into water for slurry dispersion.
[0059] According to the present invention, there is no particular limitation on the method of mixing and slurrying the active metal precursor with the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and optionally the precursor of the precious metal component, and there is no limitation on the order of adding the active metal precursor with the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and optionally the precursor of the precious metal component, as long as the active metal precursor is contacted with the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and optionally the precursor of the precious metal component and water. When the slurrying process also contains a precious metal component precursor, the specific mixing and slurrying process may include: adding the precious metal component precursor (which may be introduced in the form of a solution) to the acidified inorganic oxide matrix for mixing and slurrying, then adding the active metal precursor, and then drying and / or calcining the slurry to obtain a finished catalyst.
[0060] According to the present invention, preferably, the solid content of the slurry in step (2) is 5-40% by weight.
[0061] The drying in step (2) is preferably spray drying. In the present invention, the spray drying can be carried out according to conventional technical means in the art, and the present invention has no particular limitation thereto. Those skilled in the art can select appropriate spray drying conditions according to the average particle size of the target catalyst, and preferably the spray drying conditions are such that the average particle size of the particles obtained by spray drying is 60-80 μm, and the particle size distribution range is mainly 20-100 μm.
[0062] Preferably, the calcination conditions in step (2) include: temperature of 300-800° C. and time of 1-5 h.
[0063] According to the preparation method of the present invention, there is no particular limitation on the impregnation in step (3), which can be carried out according to conventional techniques in the art, and can be saturated impregnation or excessive impregnation, preferably excessive impregnation.
[0064] According to the present invention, preferably, in step (3), the noble metal component precursor is hydrolyzed in an acid solution to provide the impregnation solution. Specifically, after the hydrolysis, dilution (water may be added) or concentration (evaporation may be performed) may be performed, and then the impregnation is performed to provide a catalyst with a specific noble metal component loading.
[0065] Preferably, the acid is selected from water-soluble inorganic acids and / or organic acids, preferably at least one selected from hydrochloric acid, nitric acid, phosphoric acid and acetic acid.
[0066] According to the present invention, preferably, the amount of the acid used is such that the pH value of the impregnation solution is less than 6.0, preferably less than 5.0. This preferred embodiment is more conducive to uniform dispersion of active components and improvement of the wear resistance of the finished catalyst.
[0067] The present invention can obtain the solid product by filtering the mixture obtained after the immersion. The filtration can be performed according to conventional technical means in the art.
[0068] In step (3) of the present invention, the solid product may be dried only, or calcined only, or the solid product may be dried and then calcined. The present invention has no particular limitation on this. Preferably, the solid product is dried and then calcined. The present invention has no particular limitation on the conditions for drying and calcining, and they may be carried out according to conventional technical means in the art. For example, the drying conditions may include: a temperature of 60-150°C and a time of 2-10h. The present invention has no particular limitation on the conditions for calcining, and the calcination may be carried out in air or an inert atmosphere (such as nitrogen). The present invention has no particular limitation on this. The conditions for calcining in step (3) preferably include: a temperature of 300-800°C and a time of 0.1-5h.
[0069] The catalyst provided by the present invention is suitable for any SO x and NO x It is especially suitable for removing SO from catalytic cracking regeneration flue gas. x and NO x Based on this, the third aspect of the present invention provides a catalyst prepared by the catalyst described in the first aspect and the preparation method described in the second aspect for simultaneously removing SO from catalytic cracking regeneration flue gas. x and NO x Application in reaction.
[0070] A fourth aspect of the present invention provides a method for simultaneously removing SO from flue gas. x and NO x The method comprises: removing SO x and NO x Under the conditions of SO x and NO x The flue gas is contacted with the catalyst described in the first aspect and the catalyst prepared by the preparation method described in the second aspect.
[0071] Preferably, the de-SO x and NO x The conditions include: temperature of 500-800℃, pressure of 0.02-4MPa, volumetric air velocity of flue gas of 100-50000h -1 Further preferably, the temperature is 550-780°C, the pressure is 0.03-2MPa, and the volumetric air velocity of the flue gas is 200-20000h -1 In the present invention, unless otherwise specified, the pressure is a gauge pressure.
[0072] The present invention treats SO in the flue gasx and NO x The content selection range is wide, as long as it contains SO x and NO x That is, it is conducive to the removal of the two. Preferably, in the flue gas, SO x The content is 0.001-0.5% by volume, NO x The content of SO in the flue gas is 0.001-0.3 volume %; further preferably, SO x The content is 0.002-0.2% by volume, NO x The content is 0.002-0.2 volume %.
[0073] Preferably, in the flue gas, SO x with NO x The volume content ratio of is 1-1.4: 1, preferably 1-1.2: 1. This preferred embodiment is more conducive to improving the removal efficiency of the two.
[0074] Preferably, the flue gas is catalytic cracking regeneration flue gas. In addition to SO x and NO x In addition, it may also contain CO, CO2, and H2O components.
[0075] In the present invention, unless otherwise specified, ppm refers to volume concentration.
[0076] The implementation process of the present invention and the beneficial effects produced are described in detail below through specific embodiments, aiming to help readers more clearly understand the spirit and essence of the present invention, but shall not constitute any limitation on the scope of implementation of the present invention.
[0077] In the following examples, the method is used to simultaneously reduce SO in flue gas. x with NO x The content of the components in the catalyst was determined by X-ray fluorescence spectroscopy (XRF), see Analytical Methods for Petrochemical Industry (RIPP Experimental Method), edited by Yang Cuiding et al., Science Press, 1990. Raw materials used in comparative examples and examples: lanthanum nitrate (analytical grade, Aladdin Biochemical Company), magnesium nitrate (analytical grade, Sinopharm Chemical Reagent Co., Ltd.), manganese chloride (analytical grade, Beijing Chemical Plant), cobalt nitrate (analytical grade, Beijing Inokai Technology Co., Ltd.), ammonium carbonate (analytical grade, Beijing Chemical Plant), ammonia (analytical grade, 25%, Tianjin Damao Chemical Plant), palladium chloride (Beijing Purchasing and Supply Station of China Pharmaceutical Company), hydrochloric acid (Beijing Chemical Plant), OX50-SiO2 (Sinopec Catalyst Company).
[0078] Example 1
[0079] Weigh 420 mL of deionized water in a beaker, add 30 g of lanthanum nitrate based on the mass of La2O3, 4 g of magnesium nitrate based on the mass of MgO, 5 g of cobalt nitrate based on the mass of Co2O3, and 3 g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh 63 g of ammonium carbonate and dissolve it in 250 mL of deionized water, stir until fully dissolved, add the metal nitrate mixed solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the completely precipitated mixture and rinse with deionized water. Dry the filter cake mixture obtained by filtration at 120°C, roast it at 700°C in air atmosphere for 6 hours, and grind it to obtain an active metal precursor.
[0080] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200°C, and calcine at 700°C in air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of the non-precious metal active component in the prepared microsphere catalyst semi-finished product is 33%.
[0081] Weigh the palladium precursor and dilute hydrochloric acid in a mass ratio of 1:1, dilute with deionized water, and prepare a palladium chloride solution with a concentration of 5.6g / L and a pH of 2. Weigh 15g of the catalyst microsphere semi-finished product, and weigh a certain amount of palladium chloride solution with a concentration of 5.6g / L based on the palladium mass of 0.0045g. The palladium chloride solution is used as an impregnation liquid to impregnate the above-mentioned catalyst microsphere semi-finished product to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours to obtain catalyst S-1.
[0082] Example 2
[0083] Weigh 250 mL of deionized water in a beaker, add 10 g of lanthanum nitrate based on the mass of La2O3, 7 g of magnesium nitrate based on the mass of MgO, 5 g of cobalt nitrate based on the mass of Co2O3, and 3 g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh 37.5 g of ammonium carbonate and dissolve it in 150 mL of deionized water, stir until fully dissolved, add the metal nitrate mixed solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the completely precipitated mixture and rinse with deionized water. Dry the filter cake mixture obtained by filtration at 120°C, roast it at 700°C in an air atmosphere for 6 hours, and grind it to obtain an active metal precursor.
[0084] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 10 g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200°C, and calcine at 700°C in air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of the non-precious metal active component in the prepared microsphere catalyst semi-finished product is 20%.
[0085] Weigh the palladium precursor and dilute hydrochloric acid in a mass ratio of 1:1, dilute with deionized water, and prepare a palladium chloride solution with a concentration of 5.6g / L and a pH of 2. Weigh 15g of the catalyst microsphere semi-finished product, and weigh a certain amount of palladium chloride solution with a concentration of 5.6g / L based on the palladium mass of 0.0030g. The palladium chloride solution is used as an impregnation liquid to impregnate the above-mentioned catalyst microsphere semi-finished product to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours. The obtained catalyst is recorded as S-2.
[0086] Example 3
[0087] Weigh 410 mL of deionized water in a beaker, add 30 g of lanthanum nitrate based on the mass of La2O3, 5 g of magnesium nitrate based on the mass of MgO, 2.6 g of cobalt nitrate based on the mass of Co2O3, and 3.4 g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh 61.5 g of ammonium carbonate and dissolve it in 250 mL of deionized water, stir until fully dissolved, add the metal nitrate mixed solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the completely precipitated mixture and rinse with deionized water. Dry the filter cake mixture obtained by filtration at 120°C, roast it at 700°C in air atmosphere for 6 hours, and grind it to obtain an active metal precursor.
[0088] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200°C, and calcine at 700°C in air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of the non-precious metal active component in the prepared microsphere catalyst semi-finished product is 33%.
[0089] Weigh the palladium precursor and dilute hydrochloric acid in a mass ratio of 1:1, dilute with deionized water, and prepare a palladium chloride solution with a concentration of 5.6g / L and a pH of 2. Weigh 15g of the catalyst microsphere semi-finished product, and weigh a certain amount of palladium chloride solution with a concentration of 5.6g / L based on the palladium mass of 0.0030g. The palladium chloride solution is used as an impregnation liquid to impregnate the above-mentioned catalyst microsphere semi-finished product to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours. The obtained catalyst is recorded as S-3.
[0090] Example 4
[0091] The method of Example 1 is followed, except that the amount of aluminum ore is reduced and the mass percentage of the non-precious metal active components in the prepared microsphere catalyst semi-finished product is adjusted to 50%.
[0092] Specifically, 420 mL of deionized water was weighed in a beaker, and 30 g of lanthanum nitrate, 4 g of magnesium nitrate, 5 g of cobalt nitrate and 3 g of manganese chloride were added under stirring until they were completely dissolved. 63 g of ammonium carbonate was weighed and dissolved in 250 mL of deionized water, and stirred until fully dissolved. The metal nitrate mixed solution was added to the ammonium carbonate solution under stirring, and a certain amount of ammonia water was added to maintain the pH value of the solution at 9. The completely precipitated mixture was filtered and rinsed with deionized water. The filter cake mixture obtained by filtration was dried at 120°C, and after being roasted at 700°C in an air atmosphere for 6 hours, it was ground to obtain an active metal precursor.
[0093] Weigh 20 g of aluminum ore in terms of Al2O3 mass, add 240 mL of water and 3 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200° C., and calcine at 700° C. in an air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of the non-precious metal active component in the prepared microsphere catalyst semi-finished product is 50%.
[0094] Weigh the palladium precursor and dilute hydrochloric acid in a mass ratio of 1:1, dilute with deionized water, and prepare a palladium chloride solution with a concentration of 5.6g / L and a pH of 2. Weigh 15g of the catalyst microsphere semi-finished product, and weigh a certain amount of palladium chloride solution with a concentration of 5.6g / L based on the palladium mass of 0.0060g. The palladium chloride solution is used as an impregnation liquid to impregnate the above-mentioned catalyst microsphere semi-finished product to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours to obtain catalyst S-4.
[0095] Example 5
[0096] Weigh 420 mL of deionized water in a beaker, add 34 g of lanthanum nitrate based on the mass of La2O3, 4 g of magnesium nitrate based on the mass of MgO, 1 g of cobalt nitrate based on the mass of Co2O3, and 3 g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh 63 g of ammonium carbonate and dissolve it in 250 mL of deionized water, stir until fully dissolved, add the metal nitrate mixed solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the completely precipitated mixture and rinse with deionized water. Dry the filter cake mixture obtained by filtration at 120°C, roast it at 700°C in air atmosphere for 6 hours, and grind it to obtain an active metal precursor.
[0097] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200°C, and calcine at 700°C in air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of the non-precious metal active component in the prepared microsphere catalyst semi-finished product is 33%.
[0098] Weigh the palladium precursor and dilute hydrochloric acid in a mass ratio of 1:1, dilute with deionized water, and prepare a palladium chloride solution with a concentration of 5.6g / L and a pH of 2. Weigh 15g of the catalyst microsphere semi-finished product, and weigh a certain amount of palladium chloride solution with a concentration of 5.6g / L based on the palladium mass of 0.0030g. The palladium chloride solution is used as an impregnation liquid to impregnate the above-mentioned catalyst microsphere semi-finished product to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours to obtain catalyst S-5.
[0099] Example 6
[0100] Weigh 510 mL of deionized water in a beaker, add 22 g of lanthanum nitrate based on the mass of La2O3, 4 g of magnesium nitrate based on the mass of MgO, 22 g of cobalt nitrate based on the mass of Co2O3, and 3 g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh 76.5 g of ammonium carbonate and dissolve it in 300 mL of deionized water, stir until fully dissolved, add the metal nitrate mixed solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the completely precipitated mixture and rinse with deionized water. Dry the filter cake mixture obtained by filtration at 120°C, roast it at 700°C in air atmosphere for 6 hours, and grind it to obtain an active metal precursor.
[0101] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200°C, and calcine at 700°C in air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of the non-precious metal active component in the prepared microsphere catalyst semi-finished product is 33%.
[0102] Weigh the palladium precursor and dilute hydrochloric acid in a mass ratio of 1:1, dilute with deionized water, and prepare a palladium chloride solution with a concentration of 5.6g / L and a pH of 2. Weigh 15g of the catalyst microsphere semi-finished product, and weigh a certain amount of palladium chloride solution with a concentration of 5.6g / L based on the palladium mass of 0.0045g. The palladium chloride solution is used as an impregnation liquid to impregnate the above-mentioned catalyst microsphere semi-finished product to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours to obtain catalyst S-6.
[0103] Example 7
[0104] Weigh 420 mL of deionized water in a beaker, add 30 g of lanthanum nitrate based on the mass of La2O3, 4 g of magnesium nitrate based on the mass of MgO, 5 g of cobalt nitrate based on the mass of Co2O3, and 3 g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh 63 g of ammonium carbonate and dissolve it in 250 mL of deionized water, stir until fully dissolved, add the metal nitrate mixed solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the completely precipitated mixture and rinse with deionized water. Dry the filter cake mixture obtained by filtration at 120°C, roast it at 700°C in air atmosphere for 6 hours, and grind it to obtain an active metal precursor.
[0105] Weigh 40g of aluminum ore in terms of Al2O3 mass, add 380mL of water and 6g of 36% by weight concentrated hydrochloric acid, and slurry. Weigh 20g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200°C, and calcine it for a second time at 700°C in air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of non-precious metal active components in the prepared microsphere catalyst semi-finished product is 33%.
[0106] Weigh the precursor of ruthenium and dissolve it in dilute hydrochloric acid in a ratio of 1:1, add deionized water to dilute it, and prepare a ruthenium chloride solution with a concentration of 5.6g / L. Weigh 15g of the semi-finished catalyst microspheres, and weigh a certain amount of ruthenium chloride solution with a concentration of 5.6g / L according to the mass of ruthenium contained in 0.0045g. The ruthenium-containing solution is used as an impregnation liquid to impregnate the above-mentioned semi-finished catalyst to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours to obtain catalyst S-7.
[0107] Example 8
[0108] Weigh 420 mL of deionized water in a beaker, add 30 g of cerium nitrate based on the mass of CeO2, 4 g of magnesium nitrate based on the mass of MgO, 5 g of ferric nitrate based on the mass of Fe2O3, and 3 g of manganese chloride based on the mass of MnO under stirring until completely dissolved. Weigh 63 g of ammonium carbonate and dissolve it in 250 mL of deionized water, stir until fully dissolved, add the metal nitrate mixed solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the completely precipitated mixture and rinse with deionized water. Dry the filter cake mixture obtained by filtration at 120°C, roast it at 700°C in air atmosphere for 6 hours, and grind it to obtain an active metal precursor.
[0109] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Weigh 20 g of active metal precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 200°C, and calcine at 700°C in air atmosphere for 4 hours to obtain a catalyst microsphere semi-finished product. The mass percentage of the non-precious metal active component in the prepared microsphere catalyst semi-finished product is 33%.
[0110] Weigh the palladium precursor and dilute hydrochloric acid in a mass ratio of 1:1, dilute with deionized water, and prepare a palladium chloride solution with a concentration of 5.6g / L and a pH of 2. Weigh 15g of the catalyst microsphere semi-finished product, and weigh a certain amount of palladium chloride solution with a concentration of 5.6g / L based on the palladium mass of 0.0045g. The palladium chloride solution is used as an impregnation liquid to impregnate the above-mentioned catalyst microsphere semi-finished product to obtain a solid product, and then the solid product is dried at 120°C, and then calcined at 700°C in an air atmosphere for 4 hours to obtain catalyst S-8.
[0111] Comparative Example 1
[0112] Weigh 30g of lanthanum nitrate based on the mass of La2O3 and dissolve it in a beaker, weigh 45g of ammonium carbonate and completely dissolve it in a beaker, add the lanthanum nitrate solution to the ammonium carbonate solution under stirring, and add a certain amount of ammonia water to maintain the pH value of the solution at 9. Filter the mixture obtained above, dry the filter cake mixture obtained by filtration at 120°C, calcine it at 700°C in air atmosphere for 6 hours, and grind it to obtain the catalytic precursor L.
[0113] 5 g of cobalt nitrate based on the mass of Co2O3 was weighed and completely dissolved in a beaker, 7.5 g of ammonium carbonate was weighed and completely dissolved in a beaker, and the cobalt nitrate solution was added to the ammonium carbonate solution under stirring, and a certain amount of ammonia water was added to maintain the pH value of the solution at 9. The mixture obtained above was filtered, and the filter cake mixture obtained by filtration was dried at 120°C, calcined at 700°C in air atmosphere for 6 hours, and then ground to obtain active metal precursor C.
[0114] The active metal precursor L and the active metal precursor C obtained in the first two steps are fully mechanically mixed to obtain a mixed precursor.
[0115] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Take 20 g of the mixed precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 120°C, and calcine at 700°C in air atmosphere for 4 hours to obtain catalyst D-1.
[0116] Comparative Example 2
[0117] The catalyst was prepared as follows: 15 g of OX50 (SiO2) powder and a certain amount of palladium chloride solution prepared in Example 1 were weighed according to the palladium content of 0.0045 g. The palladium chloride solution was added to the OX50 powder and mixed evenly by continuous stirring. The obtained mixture was placed in an oven at 120° C. until dried, and calcined at 700° C. in an air atmosphere for 4 hours to obtain catalyst D-2.
[0118] Comparative Example 3
[0119] Weigh 30 g of La2O3 and 5 g of Co2O3, mix them mechanically thoroughly, and obtain a mixed precursor.
[0120] Weigh 40 g of aluminum ore in terms of Al2O3 mass, add 380 mL of water and 6 g of 36 wt% concentrated hydrochloric acid, and slurry. Take 20 g of the mixed precursor and add it to the acidified inorganic oxide matrix, mix and stir, dry the slurry at 120°C, and calcine at 700°C in air atmosphere for 4 hours to obtain catalyst D-3.
[0121] Comparative Example 4
[0122] Comparative catalyst D-4 was prepared by referring to the method described in CN110787834A. Alumina, kaolin, magnesium, boron, lanthanum, platinum, titanium, aluminum sol, and ethyl acetate were weighed and mixed according to the proportions in Table 1, 5 times of water was added, and the mixture was immersed at 85°C for more than 3 hours. After immersion, the mixture was stirred at 85°C for 3 hours to make it uniformly dispersed. The above slurry was spray-dried at 300°C and sieved to obtain particles of ≤200μm; the obtained particles were calcined at 500°C for 4 hours, and the obtained active metal precursor was fully ground, pressed into tablets (15MPa), and sieved to obtain the final catalyst, which was recorded as D-4.
[0123] Table 1 (Mass percentage content)
[0124] Alumina 65 Kaolin 18 magnesium 2 boron 2 lanthanum 3.5 platinum 0.5 titanium 4 Aluminum sol 4 Ethyl acetate 1
[0125] The composition of the catalyst obtained above is listed in Table 2.
[0126] Table 2 Composition of catalyst
[0127]
[0128]
[0129] Note: In Table 2, the unit of each component content is "weight %"
[0130] The catalyst activity evaluation standard in the present invention is based on the SO x and NO x As a measure of the concentration change, the SO x and NO x The content is measured by FT-IR Fourier infrared flue gas analyzer and evaluated by fixed bed microreactor experimental device. The catalyst activity evaluation result is expressed as conversion rate.
[0131] Conversion rate calculation method:
[0132]
[0133] Among them, C (inlet) Refer to the experimental device entrance SO x or NO x The concentration of C (outlet) Refers to the experimental device outlet SO x or NO x concentration.
[0134] Test Example 1
[0135] This test example is used to evaluate the effect of the catalysts provided in the above examples and comparative examples on reducing NO and SO2 emissions in flue gas at the same time. The catalytic cracking reaction-regeneration evaluation was carried out on a small fixed bed simulated flue gas device, with a catalyst loading of 1.5 g, a reaction temperature of 680°C, a pressure of 0.03 MPa, a feed gas volume flow rate (standard condition) of 1500 mL / min, and a volume space velocity of about 15000 h -1 The raw gas contained 1200 ppm NO, 1200 ppm SO2, and the balance was N2. The gas products were analyzed by an online infrared analyzer to obtain the concentrations of SO2 and NO after the reaction. The results for the evaluation time of 0.5 h are listed in Table 3, and the results for the evaluation time of 1.5 h are listed in Table 4.
[0136] Table 3 Comparison of desulfurization and denitrification performance of different catalysts within 0.5h
[0137] 0.5h total conversion rate (%) Combination-NO <![CDATA[Combination - SO2]]> Alone-NO <![CDATA[Separate - SO2]]> S-1 71 72 <2 62 S-2 50 53 <2 50 S-3 57 63 <2 60 S-4 92 78 <2 68 S-5 46 66 <2 65 S-6 31 56 <2 55 S-7 65 70 <2 60 S-8 59 72 <2 65 D-1 <2 33 <2 32 D-2 10 <2 10 <2 D-3 5 7 <2 7 D-4 4 24 5 23
[0138] Note: In Table 3, single-NO and single-SO2 refer to the feed gas containing only 1200ppm NO or 1200ppm SO2 respectively.
[0139] As can be seen from Table 3, within the first 0.5 h, the method for simultaneously reducing SO in flue gas provided by the present invention x with NO x The catalyst prepared by the present invention has a pollutant removal rate in the reaction of mixing NO and SO2 gas and a pollutant removal rate in the reaction of feeding SO2 gas alone and NO gas alone under the same evaluation conditions compared with the catalyst prepared by the prior art. This indicates that the catalyst provided by the present invention has a high catalytic conversion activity, especially the catalytic conversion activity of NO is greatly improved in the combined catalytic process.
[0140] Table 4 Comparison of desulfurization and denitrification performance of different catalysts within 1.5h
[0141]
[0142]
[0143] Note: In Table 4, single-NO and single-SO2 refer to the feed gas containing only 1200ppm NO or 1200ppm SO2 respectively.
[0144] As can be seen from Table 4, within 1.5 h, the method for simultaneously reducing SO in flue gas provided by the present invention x with NO xCompared with the catalyst prepared by the prior art under the same evaluation conditions, the pollutant removal rate of the catalyst prepared by the prior art in the reaction of mixing NO and SO2 is significantly better than that of the reaction of feeding SO2 gas alone and NO gas alone. The total conversion rate of 1.5h is slightly lower than that of 0.5h, especially in the SO2 removal conversion rate, the decrease is very small, indicating that the introduction of IIA group metal components can effectively alleviate the problem of sulfur-induced deactivation and effectively improve the reaction stability of the catalyst.
[0145] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for simultaneously reducing SO in flue gas x with NO x A catalyst characterized in that Based on the total weight of the catalyst, it contains 25-95% by weight of an inorganic oxide matrix; 2-70% by weight of a rare earth metal component calculated as oxide; 1-30% by weight of a Group IIA metal component calculated as oxide; 1-12% by weight of one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB calculated as oxide; 1-10% by weight of a Group VIIB non-precious metal component calculated as oxide; and 0.01-1.5% by weight of a precious metal component calculated as an element; The rare earth metal component is selected from one or more of lanthanum, cerium, praseodymium and neodymium; The Group IIA metal component is selected from one or more of beryllium, magnesium, calcium, strontium and barium; The one or more non-precious metal components of the VB, VIII, IB, and IIB groups are selected from one or more of iron, cobalt, nickel, copper, zinc, and vanadium; The noble metal component is selected from one or more of ruthenium, rhodium, rhenium, platinum, palladium, silver, iridium and gold.
2. The catalyst according to claim 1, wherein Based on the total weight of the catalyst, it contains 40-90 wt % of an inorganic oxide matrix; 4-50 wt % of a rare earth metal component calculated as oxide; 1-20 wt % of a Group IIA metal component calculated as oxide; 2-12 wt % of one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB calculated as oxide; 1-8 wt % of a Group VIIB non-precious metal component calculated as oxide; and 0.02-1.2 wt % of a precious metal component calculated as an element.
3. The catalyst according to claim 2, wherein Based on the total weight of the catalyst, it contains 50-80 wt % of an inorganic oxide matrix; 4-40 wt % of a rare earth metal component calculated as oxide; 2-15 wt % of a Group IIA metal component calculated as oxide; 2-10 wt % of one or more non-precious metal components selected from Groups VB, VIII, IB, and IIB calculated as oxide; 2-5 wt % of a Group VIIB non-precious metal component calculated as oxide; and 0.02-1.0 wt % of a precious metal component calculated as an element.
4. The catalyst according to claim 1, wherein The rare earth metal component is selected from lanthanum and / or cerium; The Group IIA metal component is selected from magnesium; One or more non-precious metal components of the VB, VIII, IB, and IIB groups are cobalt and / or iron; The Group VIIB non-noble metal component is manganese; The noble metal component is selected from one or more of platinum, palladium and rhodium; The inorganic oxide matrix is selected from at least one of alumina, silica-alumina, zeolite, spinel, kaolin, diatomaceous earth, perlite and perovskite.
5. The catalyst according to claim 4, wherein The noble metal component is palladium.
6. The catalyst according to claim 4, wherein The inorganic oxide matrix is aluminum oxide.
7. The catalyst according to any one of claims 1 to 6, wherein Calculated on the basis of metal elements, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from groups VB, VIII, IB, and IIB is (0.4-18):
1.
8. The catalyst according to claim 7, wherein Calculated on the basis of metal elements, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from the VB, VIII, IB, and IIB groups is (0.5-12):
1.
9. The catalyst according to claim 8, wherein Calculated on the basis of metal elements, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from groups VB, VIII, IB, and IIB is (1-6):
1.
10. A method for simultaneously reducing SO in flue gas x with NO x A method for preparing a catalyst, the method comprising the following steps: (1) Obtaining active metal precursors by coprecipitation or sol-gel method; (2) mixing and slurrying the active metal precursor with the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and optionally the precious metal component precursor to obtain a slurry, and drying and / or calcining the slurry to obtain a composition; The method may further optionally include: (3) impregnating the composition obtained in step (2) with a solution containing a noble metal component precursor as an impregnation solution to obtain a solid product, and then drying and / or calcining the solid product; The active metal in the active metal precursor includes a rare earth metal component, a IIA group metal component, one or more non-precious metal components selected from VB, VIII, IB, and IIB groups, and a VIIB group non-precious metal component; The active metal precursor, the inorganic oxide matrix and / or the precursor of the inorganic oxide matrix and the noble metal component precursor are used in such amounts that the prepared catalyst contains, based on the total weight of the catalyst, 25-95 wt % of the inorganic oxide matrix; 2-70 wt % of the rare earth metal component in terms of oxide; 1-30 wt % of the IIA group metal component in terms of oxide; 1-12 wt % of one or more non-noble metal components selected from the VB, VIII, IB and IIB groups in terms of oxide; 1-10 wt % of the VIIB group non-noble metal component in terms of oxide; and 0.01-1.5 wt % of the noble metal component in terms of element. The rare earth metal component is selected from one or more of lanthanum, cerium, praseodymium and neodymium; The Group IIA metal component is selected from one or more of beryllium, magnesium, calcium, strontium and barium; The one or more non-precious metal components of the VB, VIII, IB, and IIB groups are selected from one or more of iron, cobalt, nickel, copper, zinc, and vanadium; The noble metal component is selected from one or more of ruthenium, rhodium, rhenium, platinum, palladium, silver, iridium and gold.
11. The preparation method according to claim 10, wherein: The active metal precursor, inorganic oxide matrix and / or inorganic oxide matrix precursor and precious metal component precursor are used in such amounts that the prepared catalyst contains, based on the total weight of the catalyst, 40-90 wt % of inorganic oxide matrix; 4-50 wt % of rare earth metal components calculated as oxides; 1-20 wt % of Group IIA metal components calculated as oxides; 2-12 wt % of one or more non-precious metal components selected from Groups VB, VIII, IB and IIB calculated as oxides; 1-8 wt % of Group VIIB non-precious metal components calculated as oxides; and 0.02-1.2 wt % of precious metal components calculated as elements.
12. The preparation method according to claim 11, wherein The active metal precursor, inorganic oxide matrix and / or inorganic oxide matrix precursor and precious metal component precursor are used in such amounts that the prepared catalyst contains, based on the total weight of the catalyst, 50-80 wt % of inorganic oxide matrix; 4-40 wt % of rare earth metal components calculated as oxides; 2-15 wt % of Group IIA metal components calculated as oxides; 2-10 wt % of one or more non-precious metal components selected from Groups VB, VIII, IB and IIB calculated as oxides; 2-5 wt % of Group VIIB non-precious metal components calculated as oxides; and 0.02-1.0 wt % of precious metal components calculated as elements.
13. The preparation method according to any one of claims 10 to 12, wherein: In the active component precursor, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from VB, VIII, IB, and IIB groups is (0.4-18):1, calculated as metal elements.
14. The preparation method according to claim 13, wherein: In the active component precursor, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from VB, VIII, IB, and IIB groups is (0.5-12):1, calculated as metal elements.
15. The preparation method according to claim 14, wherein: In the active component precursor, the molar ratio of the rare earth metal component to one or more non-precious metal components selected from VB, VIII, IB, and IIB groups is (1-6):1, calculated as metal elements.
16. The preparation method according to claim 10, wherein: The rare earth metal component is lanthanum and / or cerium; The Group IIA metal component magnesium; One or more non-precious metal components of the VB, VIII, IB, and IIB groups are cobalt and / or iron; The Group VIIB non-noble metal component is manganese; The noble metal component is selected from one or more of platinum, palladium and rhodium; The inorganic oxide matrix is selected from at least one of alumina, silica-alumina, zeolite, spinel, kaolin, diatomaceous earth, perlite and perovskite.
17. The preparation method according to claim 16, wherein: The noble metal component is selected as palladium.
18. The preparation method according to claim 16, wherein: The inorganic oxide matrix is aluminum oxide.
19. The preparation method according to claim 10, wherein: In step (1), the active metal precursor is obtained by a co-precipitation method.
20. The preparation method according to claim 19, wherein: The coprecipitation method comprises: (1-1) providing a first solution containing a rare earth metal component precursor, a Group IIA metal component precursor, one or more non-noble metal component precursors selected from Groups VB, VIII, IB, and IIB, and a Group VIIB non-noble metal component precursor; (1-2) subjecting the first solution to a coprecipitation reaction with a coprecipitant; (1-3) Drying and / or calcining the solid product obtained by the coprecipitation reaction.
21. The preparation method according to claim 20, wherein: The rare earth metal component precursor, the IIA group metal component precursor, one or more non-precious metal component precursors selected from groups VB, VIII, IB, and IIB, and the VIIB group non-precious metal component precursor can be independently selected from the nitrate and / or chloride of each metal component.
22. The preparation method according to claim 20, wherein: The coprecipitant is carbonate.
23. The preparation method according to claim 22, wherein: The coprecipitant is selected from at least one of ammonium carbonate, potassium carbonate and sodium carbonate.
24. The preparation method according to claim 20, wherein: The coprecipitation reaction is carried out at a pH of 8-10.
25. The preparation method according to claim 20, wherein: The calcination conditions in step (1-3) include: temperature of 300-800°C and time of 1-8h.
26. The preparation method according to claim 10, wherein: The solid content of the slurry in step (2) is 5-40% by weight.
27. The preparation method according to claim 10, wherein: The calcination conditions in step (2) include: temperature of 300-800° C. and time of 1-5 h.
28. The preparation method according to claim 10, wherein: In step (3), the noble metal component precursor is hydrolyzed in an acid solution to provide the impregnation solution.
29. The preparation method according to claim 28, wherein The acid is selected from inorganic acids and / or organic acids soluble in water.
30. The preparation method according to claim 29, wherein: The acid is selected from at least one of hydrochloric acid, nitric acid, phosphoric acid and acetic acid.
31. The preparation method according to claim 28, wherein The acid is used in an amount such that the pH of the impregnation solution is less than 6.
0.
32. The preparation method according to claim 31, wherein The acid is used in an amount such that the pH of the impregnation solution is less than 5.
0.
33. The preparation method according to claim 10, wherein: The calcination conditions in step (3) include: temperature of 300-800°C and time of 0.1-5h.
34. The catalyst according to any one of claims 1 to 9 or the catalyst prepared by the preparation method according to any one of claims 10 to 33 is used for removing SO in catalytic cracking regeneration flue gas x and NO x Application in reaction.
35. Remove SO from flue gas simultaneously x and NO x methods, including: In the removal of SO x and NO x Under the conditions of SO x and NO x The flue gas is contacted with the catalyst described in any one of claims 1 to 9 or the catalyst prepared by the preparation method described in any one of claims 10 to 33.
36. The method of claim 35, wherein: The SO removal x and NO x The conditions include: temperature of 500-800℃, pressure of 0.02-4MPa, volumetric air velocity of flue gas of 100-50000h -1 .
37. The method of claim 35, wherein: In the flue gas, SO x The content of NO is 0.001-0.5% by volume x The content is 0.001-0.3 volume %.
38. The method of claim 37, wherein: The flue gas is catalytic cracking regeneration flue gas.