A star-shaped phosphate-based water reducer and preparation method thereof
The star-shaped phosphate-based water-reducing agent prepared by the reaction of star-shaped monomers with phosphorylation solves the problem of insufficient adaptability of polycarboxylate water-reducing agents, and achieves high water reduction rate, low dosage and good slump retention performance, thereby reducing preparation cost and improving environmental friendliness.
Patent Information
- Application Number
- CN202211548758.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing polycarboxylate superplasticizers have compatibility issues in concrete, resulting in poor fluidity, significant slump loss, and an unfriendly preparation process that increases usage costs.
A modified star-shaped tannic acid intermediate C is generated by esterification of star-shaped monomers A and B, and then phosphorylated with phosphorylating reagent D to prepare a star-shaped phosphate-based water-reducing agent. This process controls the molecular structure, simplifies the preparation process, and reduces costs.
The prepared star-shaped phosphate-based water-reducing agent has high water reduction rate, low dosage, good slump retention performance and anti-mud sensitivity, strong adaptability, and is suitable for various cements. It is also green and environmentally friendly.
Smart Images

Figure CN115772261B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete admixtures in building materials, and specifically relates to a preparation method of a highly adaptable star-shaped phosphate-based water reducer. Background Art
[0002] With the construction of infrastructure in my country, polycarboxylate water reducer has been widely used in nuclear power, water conservancy, high-speed rail, subway, bridges, tunnels, etc. due to its many advantages such as low dosage, high water reduction rate, excellent slump retention performance, low shrinkage, energy saving and environmental protection, but at the same time, some problems have been exposed. In actual engineering use, polycarboxylate water reducer often has compatibility problems with cement, machine-made sand, mineral admixtures such as fly ash and mineral powder. In addition, the mud content in sand and gravel has a significant impact on the performance of polycarboxylate water reducer, resulting in poor concrete fluidity and large slump loss, which greatly restricts the promotion and application of polycarboxylate water reducer.
[0003] At present, the adaptability problem is mainly manifested in that the slump does not meet the design requirements or the slump loss over time is too large, and may even cause abnormal coagulation such as rapid coagulation and false coagulation or serious bleeding, which ultimately leads to the decline of concrete mechanical properties and durability. The compatibility problem with concrete constituent materials not only increases the difficulty of the construction control process of using polycarboxylate water reducer, but also greatly increases the cost of using polycarboxylate water reducer in concrete, which has a great negative impact on the wide application of polycarboxylate water reducer in engineering. Therefore, it is necessary to research and develop new water reducers to solve the above problems.
[0004] Chinese patent CN107337766A introduces a highly adaptable polycarboxylate water reducer, which is prepared by free radical copolymerization of acrylic acid, polyether macromonomer, functional polycationic macromonomer and unsaturated phosphate monomer, wherein the polycationic group in the polycarboxylate water reducer can effectively inhibit the influence of clay on the main chain of the polycarboxylate water reducer. However, the introduction of functional polycationic macromonomer into the polycarboxylate water reducer is expensive and not suitable for large-scale promotion and application.
[0005] Chinese patent CN103333300A introduces a star-shaped polycarboxylic acid water reducer prepared by free radical copolymerization of star-shaped cyclodextrin acrylate as the core and acrylic acid, polyethylene glycol monomethyl ether acrylate and sodium methacrylic acid sulfonate as monomers. The star-shaped cyclodextrin acrylate is prepared by the reaction of β-cyclodextrin and acryloyl chloride in the solvent DMF, and post-treatment with ether. Therefore, the preparation process uses volatile acryloyl chloride and toxic DMF and ether, which is not green and environmentally friendly.
[0006] Chinese patent CN107987271A introduces a method for preparing a low molecular weight water reducer containing a phosphate ester group: firstly, a low molecular weight chlorinated polyether is reacted with an aminating agent to obtain an aminated polyether, which is then subjected to a hyperbranching modification and then subjected to a Mannich reaction with phosphorous acid to finally obtain a terminal hyperbranched phosphate ester-based low molecular weight water reducer. The preparation process of this type of water reducer is slightly cumbersome, and the degree of reaction is difficult to control; in addition, chloride ions are introduced during the reaction process, which increases the risk of concrete freeze-thaw and steel corrosion, which is not conducive to the application of this type of water reducer.
[0007] Chinese patent CN115215982A introduces a low-sensitivity phosphate-based water reducer and its preparation method, which is obtained by polycondensing high molecular weight branched polyether, branched polyether phosphate and aldehyde monomer under acid catalysis. The preparation steps are simple, the reaction is efficient, and the molecular structure is controllable. The water reducer has a good slump-preserving effect, good adaptability to different cements, and low sensitivity to clay. However, aldehyde substances such as formaldehyde and acetaldehyde are used in the preparation process, which will remain in the water reducer and cause harm to the environment.
[0008] In summary, it is very necessary to provide a water reducing agent with low synthetic dosage, high water reduction rate, small slump loss and strong adaptability. Summary of the invention
[0009] In order to solve the above technical problems, the present invention provides a method for preparing a highly adaptable star-shaped phosphate-based water reducer, which can effectively improve the water-reducing dispersibility, mud resistance and anti-sensitivity, while reducing costs, improving efficiency and being green and environmentally friendly.
[0010] In order to achieve the above object, the present invention is achieved through the following technical solutions:
[0011] The present invention provides a method for preparing a star-shaped phosphate-based water reducer, which comprises esterifying a star-shaped monomer A and a monomer B to generate a modified star-shaped tannic acid intermediate C, and then reacting the intermediate C with a phosphorylation reagent D to obtain the star-shaped phosphate-based water reducer of the present invention, wherein the structural formula is shown in (I):
[0012]
[0013] R:H,-PH 2 O 3 ,
[0014] R1:H,CH 3 , C 12 H 25 , C 18 H 35 (I);
[0015] The three groups represented by R are H, -PH 2 O 3 , The numbers of atoms in a star-shaped phosphate-based water-reducing agent molecular formula are x, y, and z respectively; and the conditions of x+y+z=25, 0≤x≤21, 1≤y≤20, 3≤z≤10 are satisfied; wherein m=20-115;
[0016] Preferably: the molar ratio of monomer A to monomer B in the esterification reaction is 1:3 to 1:10;
[0017] Preferably: the molar ratio of intermediate C to phosphorylation reagent D in the phosphorylation reaction is 1:1 to 1:20;
[0018] Preferably: the star-shaped monomer A is tannic acid;
[0019] Preferably: monomer B is (monomethoxy) polyethylene glycol monocarboxylic acid or fatty alcohol polyoxyethylene ether carboxylic acid;
[0020] Preferably: (monomethoxy) polyethylene glycol monocarboxylic acid refers to polyethylene glycol monocarboxylic acid (PEG-COOH) or monomethoxy polyethylene glycol monocarboxylic acid (mPEG-COOH), with a molecular weight Mw of 1000 to 5000;
[0021] Preferred: fatty alcohol polyoxyethylene ether carboxylic acid is lauryl alcohol polyoxyethylene ether carboxylic acid, with the molecular formula C 12 H 25 O(CH 2 CH 2 O) n CH 2 COOH, n = 3, 4, 7, 9; or octadecyl alcohol polyoxyethylene ether carboxylic acid, molecular formula C 18 H 37 O(CH 2 CH 2 O) n CH 2 COOH, n = 3, 4, 7, 9;
[0022] Preferably, the phosphorylation reagent D is selected from any one of phosphoric acid, polyphosphoric acid, phosphorus pentoxide and pyrophosphoric acid.
[0023] The weight average molecular weight of the star-shaped phosphate-based water reducer of the present invention is in the range of 10,000 to 100,000. If the weight average molecular weight is too large or too small, the water reduction and slump retention performances will be deteriorated.
[0024] The present invention provides a method for preparing the star-shaped phosphate-based water reducer, and the specific steps are as follows:
[0025] The star-shaped monomer A and monomer B are heated to 70°C under nitrogen protection, and after adding catalyst E, the temperature is slowly raised to 100-130°C and kept constant for 3-7 hours to obtain a modified star-shaped tannic acid intermediate C; then, phosphorylation reagent D is added to intermediate C at 50-75°C, the temperature is slowly raised to 100-140°C and kept constant for 3-10 hours to obtain a star-shaped phosphate-based water reducer.
[0026] Preferably, the catalyst E is selected from any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, and ethylsulfonic acid, or any combination of two of them in any proportion, and its usage is 0.5-3% of the total mass of monomer A and monomer B.
[0027] The beneficial effects of the present invention are as follows: the preparation method of the water reducer of the present invention is simple, the production cost is low, the molecular structure is controllable, and the prepared star-shaped phosphate-based water reducer has low dosage, high water reduction rate, good collapse retention performance, and good cement adaptability and anti-mud sensitivity performance;
[0028] The star-shaped phosphate-based water reducer of the present invention can be used alone or in combination with aminosulfonic acid-based water reducers, polycarboxylic acid water reducers, etc. on the market. It can also be added with air entraining agents, retarders, early strength agents, thickening and water-retaining agents, retarders and defoamers for compound use. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a comparison chart of the pure slurry test conducted by Conch Cement.
[0030] Figure 2 This is a comparison chart of the pure paste test of Onoda cement.
[0031] Figure 3 This is a comparison chart of the pure slurry test conducted by Helin Cement. DETAILED DESCRIPTION
[0032] The following will disclose the embodiments of the present invention with drawings. For the purpose of clear description, many practical details will be described together in the following description. However, it should be understood that these practical details should not be used to limit the present invention. That is, in some embodiments of the present invention, these practical details are not necessary. In addition, for the purpose of simplifying the drawings, some conventional structures and components will be depicted in a simple schematic manner in the drawings.
[0033] The present invention provides a star-shaped phosphoric acid-based water reducer and a preparation method thereof. The star-shaped phosphoric acid-based water reducer is prepared by esterifying a star-shaped monomer A and a monomer B to generate a modified star-shaped tannic acid intermediate C, and the modified star-shaped tannic acid intermediate C undergoes a phosphorylation reaction with a phosphorylation reagent D. The specific steps are: heating the star-shaped monomer A and the monomer B to 70° C. under nitrogen protection, adding a catalyst E, slowly heating the temperature to 100-130° C., and keeping the temperature constant for 3-7 hours to obtain the modified star-shaped tannic acid intermediate C, and then adding the phosphorylation reagent D to the modified star-shaped tannic acid intermediate C at 50-75° C., slowly heating the temperature to 100-140° C., and keeping the temperature constant for 3-10 hours to obtain the star-shaped phosphoric acid-based water reducer.
[0034] The raw materials used in the examples are listed in Table 1, as follows:
[0035] Table 1 Compound codes in the synthetic examples
[0036]
[0037] Example 1
[0038] Under nitrogen protection, 1 mol of star-shaped monomer A and 3 mol of monomer B-1 are heated to 70°C, and after adding catalyst E-1, the temperature is slowly raised to 100°C and kept constant for 3 hours to obtain a modified star-shaped tannic acid intermediate C-1. Then, 1 mol of phosphorylation reagent D-1 is added to the intermediate C-1 at 50°C, the temperature is slowly raised to 100°C, and the temperature is kept constant for 3 hours to obtain a star-shaped phosphate-based water reducer P-1, wherein the catalyst E-1 is 0.5% of the mass of monomer A and monomer B.
[0039] Example 2
[0040] 1 mol of star-shaped monomer A and 5 mol of monomer B-2 were heated to 80°C under nitrogen protection, and after adding catalyst E-2, the temperature was slowly raised to 130°C and kept constant for 7 hours to obtain a modified star-shaped tannic acid intermediate C-2. Then, 7 mol of phosphorylation reagent D-2 was added to the intermediate C-2 at 75°C, the temperature was slowly raised to 140°C, and the temperature was kept constant for 10 hours to obtain a star-shaped phosphate-based water reducer P-2, wherein the catalyst E-2 was 0.7% of the mass of monomer A and monomer B.
[0041] Example 3
[0042] 1 mol of star-shaped monomer A and 8 mol of monomer B-3 were heated to 70°C under nitrogen protection, and after adding catalyst E-3, the temperature was slowly raised to 120°C and kept constant for 6 hours to obtain a modified star-shaped tannic acid intermediate C-3. Then, 15 mol of phosphorylation reagent D-3 was added to the intermediate C-3 at 65°C, the temperature was slowly raised to 120°C, and the temperature was kept constant for 7 hours to obtain a star-shaped phosphate-based water reducer P-3, wherein the catalyst E-3 was 1.3% of the mass of monomer A and monomer B.
[0043] Example 4
[0044] 1 mol of monomer A and 10 mol of monomer B-4 were heated to 70°C under nitrogen protection, and after adding catalyst E-4, the temperature was slowly raised to 110°C and kept constant for 4 hours to obtain a modified star-shaped tannic acid intermediate C-4. Then, 10 mol of phosphorylation reagent D-4 was added to the intermediate C-4 at 50°C, the temperature was slowly raised to 130°C, and the temperature was kept constant for 5 hours to obtain a star-shaped phosphate-based water reducer P-4, wherein the catalyst E-4 was 3% of the mass of monomer A and monomer B.
[0045] Example 5
[0046] 1 mol of monomer A and 5 mol of monomer B-5 were heated to 70°C under nitrogen protection, and after adding catalyst E-5, the temperature was slowly raised to 130°C and kept constant for 4 hours to obtain a modified star-shaped tannic acid intermediate C-5. Then, 20 mol of phosphorylation reagent D-4 was added to the intermediate C-5 at 70°C, the temperature was slowly raised to 125°C, and the temperature was kept constant for 4 hours to obtain a star-shaped phosphate-based water reducer P-5, wherein the catalyst E-5 was 2% of the mass of monomer A and monomer B.
[0047] Example 6
[0048] 1 mol of monomer A and 10 mol of monomer B-6 were heated to 70°C under nitrogen protection, and after adding catalyst E-1, the temperature was slowly raised to 125°C and kept constant for 3 hours to obtain a modified star-shaped tannic acid intermediate C-6. Then, 8 mol of phosphorylation reagent D-3 was added to the intermediate C-6 at 60°C, the temperature was slowly raised to 135°C, and the temperature was kept constant for 5 hours to obtain a star-shaped phosphate-based water reducer P-6, wherein the catalyst E-1 was 1.5% of the mass of monomer A and monomer B.
[0049] Example 7
[0050] 1 mol of monomer A and 5 mol of monomer B-7 were heated to 70°C under nitrogen protection, and after adding catalyst E-2, the temperature was slowly raised to 115°C and kept constant for 5 hours to obtain a modified star-shaped tannic acid intermediate C-6. Then, 12 mol of phosphorylation reagent D-1 was added to the intermediate C-6 at 75°C, the temperature was slowly raised to 125°C, and the temperature was kept constant for 4 hours to obtain a star-shaped phosphate-based water reducer P-7, wherein the catalyst E-2 was 0.9% of the mass of monomer A and monomer B.
[0051] Example 8
[0052] 1 mol of monomer A and 10 mol of monomer B-8 were heated to 70°C under nitrogen protection, and after adding catalyst E-3, the temperature was slowly raised to 130°C and kept constant for 4 hours to obtain a modified star-shaped tannic acid intermediate C-8. Then, 15 mol of phosphorylation reagent D-2 was added to the intermediate C-8 at 75°C, the temperature was slowly raised to 135°C, and the temperature was kept constant for 7 hours to obtain a star-shaped phosphate-based water reducer P-8, wherein the catalyst E-3 was 2.5% of the mass of monomer A and monomer B.
[0053] Example 9
[0054] Under nitrogen protection, 1 mol of monomer A and 9 mol of monomer B-2 were heated to 70°C, and after adding catalyst E-1, the temperature was slowly raised to 120°C and kept constant for 5 hours to obtain a modified star-shaped tannic acid intermediate C-9. Then, 15 mol of phosphorylation reagent D-3 was added to the intermediate C-9 at 70°C, the temperature was slowly raised to 120°C, and the temperature was kept constant for 5 hours to obtain a star-shaped phosphate-based water reducer P-9, wherein the catalyst E-1 was 2% of the mass of monomer A and monomer B.
[0055] Example 10
[0056] 1 mol of monomer A and 7 mol of monomer B-3 were heated to 70°C under nitrogen protection, and after adding catalyst E-4, the temperature was slowly raised to 130°C and kept constant for 5 hours to obtain a modified star-shaped tannic acid intermediate C-10. Then, 10 mol of phosphorylation reagent D-1 was added to the intermediate C-9 at 65°C, the temperature was slowly raised to 125°C, and the temperature was kept constant for 4 hours to obtain a star-shaped phosphate-based water reducer P-10, wherein the catalyst E-4 was 2.5% of the mass of monomer A and monomer B.
[0057] Comparative Example 1
[0058] In a flask equipped with a stirrer, 185g of water and 275.5g of allyl polyoxyethylene ether, wherein the molecular weight of allyl polyoxyethylene ether is 2400, are stirred and heated to dissolve, and the temperature is raised to 90°C. Then, 54g of acrylic acid, 1.26g of 3-mercaptopropionic acid and 100g of water are mixed and stirred to prepare a uniform monomer aqueous solution, which is uniformly added dropwise to the flask for 3h. At the same time, an initiator solution prepared by 160g of water and 8.1g of potassium persulfate is uniformly added dropwise for 3.5h. After all the solutions are added dropwise, the temperature is kept constant for 3h to obtain a polycarboxylic acid water reducer.
[0059] Comparative Example 2
[0060] The product was synthesized according to the method shown in Example 1 of patent CN115215982A.
[0061] Application Example 1
[0062] The effects of the star-shaped phosphate-based water reducer prepared in the example, the traditional comb-shaped water reducer in comparative example 1, and the low-sensitivity phosphate-based water reducer in comparative example 2 on the fluidity of fresh cement paste and its loss over time were evaluated. The cement paste fluidity test was carried out in accordance with the GB / T8077-2000 standard, with a fixed water-cement ratio of 0.29. The experimental results are shown in Table 2.
[0063] Table 2 Effect of different water reducing agents on the fluidity of fresh cement paste and its loss over time
[0064]
[0065] Conch cement, Onoda cement and Helin cement were used for the slurry test. Figures 1 to 3 It can be seen that under the condition of 0.12% dosage, the polycarboxylate water-reducing agent synthesized in comparative example 1 has unstable flow in three types of cement. In conch cement, the initial fluidity is 235 mm, and the net slurry fluidity of 30 min is 165 mm, and the loss is extremely large; the phosphate-based water-reducing agent synthesized in comparative example 2 has better fluidity retention ability in three types of cement than the polycarboxylate water-reducing agent in comparative example 1. In Onoda cement, the initial fluidity is 263 mm, and the net slurry fluidity of 30 min is 233 mm, and the loss is relatively reduced; and the star-shaped phosphate-based water-reducing agent synthesized in the embodiment has a greater advantage in initial dispersibility and exhibits excellent slump retention performance. For example, the initial fluidity and time loss of Example 3, Example 4, and Example 7 are better than those of Comparative Example 1 and Comparative Example 2, showing the characteristics of high water reduction, high slump retention, and high adaptability.
[0066] Application Example 2
[0067] The adaptability of the star-shaped phosphate-based water reducer prepared in the example, the traditional comb-shaped water reducer in comparative example 1, and the low-sensitive phosphate-based water reducer in comparative example 2 to the mud content in cement was evaluated. The water-cement ratio was fixed at 0.29 and Conch cement was used. The results are shown in Table 3.
[0068] Table 3 Adaptability of different water reducing agents to the mud content in cement
[0069]
[0070] It can be seen from Table 3 that when the water-cement ratio is fixed at 0.29, the amount of traditional comb-type water reducer required for powders with higher mud content is greatly increased, and the dosage needs to be increased by about 60%, while for phosphate-based water reducer, the increase in dosage is significantly reduced; at the same time, the star-shaped phosphate-based water reducer in Example 4 and Example 7 has a lower dosage and smaller loss than the phosphate-based water reducer in Comparative Example 2; This shows that the star-shaped phosphate-based water reducer has a wide range of adaptability to the mud content of sand and gravel, and has outstanding advantages in overcoming the adaptability of traditional comb-type water reducers and clay-containing materials.
[0071] The water reducer preparation method of the invention is simple, the production cost is low, and the molecular structure is controllable. The prepared star-shaped phosphate-based water reducer has low dosage, high water reduction rate, good collapse retention performance, and good cement adaptability and anti-mud sensitivity performance.
[0072] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A star-shaped phosphate-based water reducer, characterized in that: The structure of the star-shaped phosphate-based water reducer conforms to the general formula (I): The three groups represented by R are H, -PH2O3, The numbers of atoms in a star-shaped phosphate-based water-reducing agent molecular formula are x, y, and z respectively; and the conditions of x+y+z=25, 0≤x≤21, 1≤y≤20, 3≤z≤10 are satisfied; wherein m=20-115.
2. A method for preparing a star-shaped phosphate-based water reducer as claimed in claim 1, characterized in that: The star-shaped phosphoric acid-based water reducer is prepared by esterifying a star-shaped monomer A and a monomer B to generate a modified star-shaped tannic acid intermediate C, and the modified star-shaped tannic acid intermediate C undergoes a phosphorylation reaction with a phosphorylation reagent D. The specific steps are: heating the star-shaped monomer A and the monomer B to 70° C. under nitrogen protection, adding a catalyst E, slowly heating the temperature to 100-130° C., and keeping the temperature constant for 3-7 hours to obtain the modified star-shaped tannic acid intermediate C, and then adding a phosphorylation reagent D to the modified star-shaped tannic acid intermediate C at 50-75° C., slowly heating the temperature to 100-140° C., and keeping the temperature constant for 3-10 hours to obtain the star-shaped phosphoric acid-based water reducer.
3. The method for preparing a star-shaped phosphate-based water reducer according to claim 2, characterized in that: The molar ratio of the star-shaped monomer A to the monomer B in the esterification reaction is 1:3 to 1:
10.
4. The method for preparing a star-shaped phosphate-based water reducer according to claim 2, characterized in that: In the phosphorylation reaction, the molar ratio of the modified star-shaped tannic acid intermediate C to the phosphorylation reagent D is 1:1 to 1:
20.
5. The method for preparing a star-shaped phosphate-based water reducer according to claim 2, characterized in that: The star-shaped monomer A is tannic acid.
6. The method for preparing a star-shaped phosphate-based water reducer according to claim 2, characterized in that: The monomer B is polyethylene glycol monocarboxylic acid or monomethoxy polyethylene glycol monocarboxylic acid or fatty alcohol polyoxyethylene ether carboxylic acid.
7. The method for preparing a star-shaped phosphate-based water reducer according to claim 6, characterized in that: The fatty alcohol polyoxyethylene ether carboxylic acid is lauryl alcohol polyoxyethylene ether carboxylic acid or octadecyl alcohol polyoxyethylene ether carboxylic acid, and the molecular formula of lauryl alcohol polyoxyethylene ether carboxylic acid is C 12 H 25 O(CH2CH2O) n CH2COOH, n = 3, 4, 7, 9, the molecular formula of octadecyl alcohol polyoxyethylene ether carboxylic acid is C 18 H 37 O(CH2CH2O) n CH2COOH, n=3,4,7,9.
8. The method for preparing a star-shaped phosphate-based water reducer according to claim 6, characterized in that: The catalyst E is any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, and ethylsulfonic acid, or a combination of two of them in any proportion. The amount of the catalyst E is 0.5-3% of the total mass of the star-shaped monomer A and the monomer B.
9. The method for preparing a star-shaped phosphate-based water reducer according to claim 2, characterized in that: The phosphorylation reagent D is one of autophosphoric acid, polyphosphoric acid, phosphorus pentoxide or pyrophosphoric acid.
10. A method for preparing a star-shaped phosphate-based water reducer according to any one of claims 2 to 9, characterized in that: The weight average molecular weight of the star-shaped phosphate-based water reducer is in the range of 10,000 to 100,000.