Processing mold and processing method of curved glass with one side bent
By designing a mold structure that combines arc and horizontal cavity, using limiting parts and temperature control, the offset problem in large-size large-arc high-curved glass molding is solved, and high-precision and efficient single-step molding is achieved.
Patent Information
- Application Number
- CN202211337988.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-10-28
AI Technical Summary
The prior art is difficult to effectively process single-sided curved glass with large sizes and large arcs, resulting in unqualified product size after forming, and multiple moldings increase costs and reduce yield.
A processing mold including upper and lower molds is designed. Through a combined structure of arc-shaped cavity and horizontal cavity, the limiting parts are used to prevent glass from being offset, and the temperature difference is controlled during thermal bending to ensure that the glass is bending. planar forming and precision.
The glass accuracy after single molding is achieved, which reduces thermal bending defects, improves production efficiency, avoids multiple processing, and solves the production problem of large-size, large-arc, high-curved glass.
Smart Images

Figure CN115784579B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass production, and in particular to a processing mold and a processing method for curved glass bent on one side. Background Art
[0002] In the process of the application and development of car curved screens, in pursuit of beauty, the design forms are becoming more and more diverse, and large-size, high-arc, and special-shaped products have appeared one after another. The existing large-size curved cover processing is mostly derived from 3D mobile phone cover technology. When faced with large-size, high-arc, and single-sided curved glass, production and processing face huge challenges. There is no mature processing technology in the market that can match various products.
[0003] At present, the curved cover with large arc height and single side bending on the vehicle is still formed by hot pressing 2D glass bending with a concave and convex graphite mold structure. However, the asymmetry of the product, the single-sided bending force, and the large amplitude will cause the glass to shift position during the molding process, resulting in NG product size after molding. The traditional solution is to reduce the amplitude of single molding through multiple molding to reduce the deviation in product molding, but this method is costly, and the product's appearance and size problems caused by multiple molding still lead to a low yield. Summary of the invention
[0004] In order to solve the above technical problem or at least partially solve the above technical problem, the present invention provides a processing mold and a processing method for curved glass that is bent on one side.
[0005] The present invention provides a processing mold for curved glass that is bent on one side. The processing mold includes an upper mold and a lower mold that are interlocked with each other. A molding cavity that matches the shape of the curved glass that is bent on one side to be molded is formed between the upper mold and the lower mold. The molding cavity includes an arc cavity and a horizontal cavity. The upper mold includes an arc mold arranged opposite to the arc cavity and a horizontal mold arranged opposite to the horizontal cavity. A limiting member is provided in the horizontal cavity for limiting the horizontal direction with the horizontal segment of the curved glass that is bent on one side.
[0006] Optionally, a groove is provided on the horizontal section of the single-side curved glass, and the limiting member includes a limiting block provided on the lower mold for being inserted into the groove.
[0007] Optionally, part of the limit block extends out of the slot, and the limit member further includes a limit slot provided on the horizontal mold into which the extended end of the limit block can be inserted.
[0008] Optionally, the lower mold includes a bottom shell and a bottom mold arranged inside the bottom shell, the top surface of the bottom mold is formed with a lower supporting surface matching the shape of the single-sided curved glass to be formed, and the top of the lower supporting surface is below the top of the bottom shell.
[0009] Optionally, the horizontal mold includes a first cover plate and a horizontal mold body arranged on a side of the first cover plate, and the horizontal cavity is formed between the horizontal mold body and a horizontal section of the bottom mold.
[0010] Optionally, plug plates are provided on both sides of the first cover plate, slots matching the plug plates are provided on both sides of the bottom shell, a first guide plate is provided on the inner side of the plug plate, and a first guide groove matching the first guide plate is provided on the bottom shell.
[0011] Optionally, the arc-shaped mold includes a second cover plate and an arc-shaped mold body arranged on a side of the second cover plate, and the arc-shaped cavity is formed between the arc-shaped mold body and the arc-shaped segment of the bottom mold.
[0012] Optionally, second guide plates are respectively provided on both sides of the arc-shaped mold body, and second guide grooves matching the second guide plates are provided on the bottom shell.
[0013] The present invention also provides a method for processing the above-mentioned single-side curved glass processing mold, the processing method comprising the following steps:
[0014] Step S1, placing the glass into the lower mold, and limiting the horizontal section of the glass by a limiting member, and then placing the horizontal mold and the arc mold above the glass respectively;
[0015] Step S2, sending the processing mold with glass into the heat bending machine for preheating, wherein the preheating temperature of the part of the glass in the horizontal cavity is 400-520°C, and the preheating temperature of the part of the glass opposite to the arc cavity is 580-680°C, so that the part of the glass is softened and formed to a semi-formed state under the gravity of the arc mold;
[0016] Step S3, after the preheating is completed, the processing mold is moved to the forming station, the part of the glass in the horizontal cavity is pressed down at a temperature of 400-520°C and the pressure is maintained, and the part of the glass opposite to the arc cavity is slowly pressed down at a temperature of 550-650°C until the part of the glass is attached to the lower mold;
[0017] Step S4, annealing and cooling the bent glass in sequence, and then trimming the shape of the glass to obtain finished glass.
[0018] Optionally, the step S4 further includes the following steps:
[0019] Step S41, moving the processing mold to the annealing zone, and keeping the processing mold at a temperature of 380-480°C and slowly cooling it down;
[0020] Step S42, the cooled processing mold is moved to a cooling station, so that the processing mold is cooled to room temperature, and the glass is taken out to obtain a semi-finished product;
[0021] Step S43, fine carving to remove the positioning area of the glass, the cutting edge is selected at the arc position, and the tangent line is extended from the arc edge to form an angle of 0-10° with the glass edge to cut the remaining material;
[0022] Step S44, polishing the sharp corners of the edges on both sides until they are smooth to obtain the desired curved glass.
[0023] Optionally, in step S2 and / or step S3, the temperature difference between the horizontal cavity and the arc cavity is ΔT1, wherein ΔT1≤180°C.
[0024] Optionally, the temperature difference between the forming temperature of the portion of glass opposite to the arc-shaped cavity in step S3 and the preheating temperature in step S2 is ΔT2, wherein 25<ΔT2<35°C.
[0025] The technical solution provided by the embodiment of the present invention has the following advantages compared with the prior art:
[0026] The present invention divides the upper mold into an arc mold and a horizontal mold, which has a small structure and light weight, thereby avoiding crushing of the glass before molding and ensuring that the horizontal cavity area always remains flat during the molding process, thereby avoiding the high-temperature bending and flattening process in the traditional method, greatly reducing hot bending defects, and the glass can be limited by a limiter during the molding process to prevent the glass from shifting, so that the molded glass has higher precision. There is no need to process the glass multiple times, and molding can be done in one time, which effectively improves the production efficiency of the glass, thereby solving the production problem of single-sided bent large-size, large-arc, and high-curved automotive glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0028] In order to more clearly illustrate the implementation mode of the present invention or the technical solution in the prior art, the drawings required for use in the implementation mode or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0029] Figure 1 It is a structural schematic diagram of the processing mold according to an embodiment of the present invention;
[0030] Figure 2 It is a structural schematic diagram of the lower mold according to an embodiment of the present invention;
[0031] Figure 3This is a schematic structural diagram of the arc mold according to an embodiment of the present invention;
[0032] Figure 4 It is a structural schematic diagram of the horizontal mold according to an embodiment of the present invention;
[0033] Figure 5 This is a schematic diagram of the glass according to an embodiment of the present invention being installed in a processing mold;
[0034] Figure 6 It is a schematic diagram of a processing mold when the glass is attached to the lower mold according to an embodiment of the present invention;
[0035] Figure 7 It is a schematic diagram of a processing mold when the glass is in a preheated state according to an embodiment of the present invention;
[0036] Figure 8 It is a schematic diagram of a processing mold when the glass according to an embodiment of the present invention is in a forming state;
[0037] Fig. 9 It is a schematic diagram of a processing mold when the glass is in an annealing state according to an embodiment of the present invention;
[0038] Fig.10 Schematic diagram of glass before processing according to an embodiment of the present invention.
[0039] Description of Reference Numerals
[0040] 1. Upper mold; 2. Lower mold; 21. Limit block; 22. Bottom shell; 23. Bottom mold; 24. Slot; 25. First guide groove; 26. Second guide groove; 3. Glass; 31. Slot; 4. Arc mold; 41. Second cover plate; 42. Arc mold body; 43. Second guide plate; 5. Horizontal mold; 51. Limit groove; 52. First cover plate; 53. Horizontal mold body; 54. Insert plate; 55. First guide plate. DETAILED DESCRIPTION
[0041] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0042] The following description sets forth many specific details to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; obviously, the implementation methods in the specification are only part of the implementation methods of the present invention, rather than all of the implementation methods.
[0043] Combination Figures 1 to 4As shown, the processing mold for the curved glass with one side bent provided in the embodiment of the present invention includes an upper mold 1 and a lower mold 2 that are interlocked with each other, that is, the upper mold 1 can be interlocked on the top of the lower mold 2. A molding cavity that matches the shape of the curved glass 3 with one side bent to be formed is formed between the upper mold 1 and the lower mold 2, so that when the molds are closed, the glass 3 above the lower mold 2 can be bent to a set shape. The molding cavity includes an arc cavity and a horizontal cavity, and the arc cavity is connected to the horizontal cavity. The upper mold 1 includes an arc mold 4 arranged opposite to the arc cavity and a horizontal mold 5 arranged opposite to the horizontal cavity, an arc cavity is formed between the arc mold 4 and the lower mold 2, a horizontal cavity is formed between the horizontal mold 5 and the lower mold 2, and the arc mold 4 and the horizontal mold 5 are separately arranged, and a limiter is provided in the horizontal cavity for limiting the horizontal direction with the horizontal section of the curved glass 3 with one side bent. Among them, the lower mold 2 opposite to the arc cavity is a convex mold surface, and the arc mold 4 has a concave mold surface, so that the set curved glass 3 can be formed. As shown Figure 5 As shown, before processing, the glass 3 is placed above the lower mold 2, and the portion of the glass 3 opposite to it is pressed by the horizontal mold 5. Figure 6 As shown, during processing, after the glass 3 is preheated and softened, it can be pressed down by the arc mold 4 so that the glass 3 is completely attached to the top of the lower mold 2.
[0044] The present invention divides the upper mold 1 into an arc mold 4 and a horizontal mold 5, which has a small structure and light weight, and can avoid crushing the glass 3 before molding. The horizontal mold 5 can continuously apply pressure to the glass 3 in the horizontal cavity, so that the horizontal cavity area always maintains a plane during the molding process, avoiding the high-temperature bending and flattening process in the traditional method, and greatly reducing hot bending defects. At the same time, the continuous pressure applied by the horizontal mold 5 to the glass 3 can also reduce the degree of glass pulling and deformation at the limiting part, and ensure the dimensional progress after molding; and the limiting part can limit the glass 3 during the molding process to prevent the glass 3 from shifting, so that the dimensional accuracy of the molded glass 3 is higher, and there is no need to perform multiple processing on the glass 3, and molding can be performed in one time, which effectively improves the production efficiency of the glass 3, thereby solving the production problem of single-sided bending, large-size, large-arc, high-curved automotive glass 3.
[0045] In some embodiments, in combination Figure 2 and Fig.10 As shown, a groove 31 is provided on the horizontal section of the curved glass 3 that is bent on one side before processing, and the limiting member includes a limiting block 21 provided on the lower mold 2 for inserting into the groove 31. When installing the glass 3, the limiting block 21 is inserted into the groove 31. Further optimized, in order to ensure the limiting effect, part of the limiting block 21 extends out of the groove 31. At this time, as shown in FIG. Figure 4 As shown, the limiting member also includes a limiting groove 51 arranged on the horizontal mold 5 for the extended end of the limiting block 21 to be inserted into, so as to further prevent the glass 3 from moving.
[0046] like Figure 2As shown, the lower mold 2 includes a bottom shell 22 and a bottom mold 23 disposed inside the bottom shell 22, and the top surface of the bottom mold 23 is formed with a lower support surface matching the shape of the curved glass 3 to be formed with one side bent, wherein the lower support surface opposite to the arc cavity is a convex surface, and the convex surface conforms to the concave surface of the formed glass 3. The top of the lower support surface is below the top of the bottom shell 22, which is convenient for placing and positioning the glass 3, and is also convenient for positioning the horizontal mold body 53 and the arc mold body 42 described below, so as to prevent the glass from being displaced due to the bending force during the forming process, resulting in unqualified dimensions of the finished product after forming.
[0047] like Figure 4 As shown, the horizontal mold 5 includes a first cover plate 52 and a horizontal mold body 53 disposed on the side of the first cover plate 52, and a horizontal cavity is formed between the horizontal mold body 53 and the horizontal section of the bottom mold 23. The plane area of the horizontal mold body 53 corresponds to the convex surface of the non-bending area of the glass 3, ensuring heat transfer to the product when pressing down, and at the same time ensuring that the glass 3 will not warp and always be in a flat shape during the pressure and heat bending process.
[0048] Further optimized, combined with Figure 2 and Figure 4 As shown, plug plates 54 are provided on both sides of the first cover plate 52, slots 24 matching the plug plates 54 are provided on both sides of the bottom shell 22, a first guide plate 55 is provided on the inner side of the plug plate 54, and a first guide groove 25 matching the first guide plate 55 is provided on the bottom shell 22. When pressed, the plug plate 54 is inserted into the slot 24, and the first guide plate 55 is inserted into the first guide groove 25, ensuring the precise fit between the horizontal mold 5 and the lower mold 2, while allowing the sliding to only be along the vertical direction, thereby increasing the accuracy of the positioning of the horizontal mold 5.
[0049] like Figure 3 As shown, the arc mold 4 includes a second cover plate 41 and an arc mold body 42 arranged on the side of the second cover plate 41, and an arc cavity is formed between the arc mold body 42 and the arc segment of the bottom mold 23, wherein the arc mold body 42 conforms to the curved area of the formed glass 3, and the arc mold 4 is hollowed out to reduce weight to prevent the glass 3 from being crushed by its own weight. Figure 2 and Figure 3 As shown, second guide plates 43 are respectively provided on both sides of the arc-shaped mold body 42, and second guide grooves 26 matching the second guide plates 43 are provided on the bottom shell 22. When pressed, the second guide plates 43 are inserted into the second guide grooves 26 to ensure that the arc-shaped mold 4 is precisely matched with the lower mold 2, while allowing the sliding to only be along the vertical direction, thereby increasing the accuracy of the positioning of the arc-shaped mold 4.
[0050] The present invention also provides a method for processing the above-mentioned single-side curved glass 3, using the above-mentioned processing mold, the processing method comprises the following steps:
[0051] Step S1, putting the glass 3 into the lower mold 2, and limiting the horizontal section of the glass 3 by a limiting member, and then placing the horizontal mold 5 and the arc mold 4 above the glass 3 respectively.
[0052] Specifically, Fig.10 As shown, the glass 3 is provided before molding, and the 2D glass 3 shape is processed by CNC precision engraving, and a groove 31 reserved for positioning is processed on the non-bending side. Figure 7 As shown, the glass 3 to be processed is in a plane shape. After being placed in the lower mold 2, the part of the glass 3 corresponding to the arc cavity is vacated. The limiting piece adopts the setting method of the above-mentioned processing mold. During installation, the limiting block 21 is inserted into the groove 31 of the glass 3. After the positioning of the glass 3 is completed, the horizontal mold 5 is pressed above the part of the glass 3 in the horizontal cavity, and the limiting block 21 is inserted into the limiting groove 51 of the horizontal mold 5. Then the arc mold 4 is placed above the part of the glass 3 corresponding to the arc cavity, and in order to reduce the pressure of the arc mold 4 on the glass 3, the interior of the arc mold 4 can be set as a cavity.
[0053] In step S2, the processing mold containing the glass 3 is sent into the heat bending machine for preheating, wherein the preheating temperature of the part of the glass 3 in the horizontal cavity is 400-520°C, and the preheating temperature of the part of the glass 3 opposite to the arc cavity is 580-680°C, so that the part of the glass 3 is softened and formed to a semi-formed state under the gravity of the arc mold 4.
[0054] Specifically, Figure 8 As shown, the mold is divided into a forming area and a non-forming area. The part corresponding to the horizontal direction is the non-forming area, and the part corresponding to the arc cavity is the forming area. The upper heating plate in the non-forming area presses down the horizontal mold 5 and maintains the shape. The bottom of the lower mold 2 is provided with a lower heating plate. The temperatures of the upper heating plate and the lower heating plate are both 400-520°C, ensuring that the temperature of the glass 3 in this area is close to the temperature of the forming area, and at the same time it is in a relatively low temperature state. The temperature is lower than the softening point of the glass 3, so that the glass 3 is in a harder state, and the surface is compressed without defects such as mold marks and concave and convex points. At the same time, it can ensure that the position of the groove 31 will not be deformed due to the pulling force generated by the pressure of the product forming area, thereby ensuring that the groove 31 is stuck in the longitudinal position of the glass 3, preventing the glass 3 from being pulled by the groove 31 when it is soft, and the deformation and displacement of the groove 31 of the glass 3. The upper heating plate in the molding area of the mold is close to the arc mold 4 for non-contact radiation heating, and the bottom of the lower mold 2 is provided with a lower heating plate (both the upper heating plate and the lower heating plate are non-contact heating to avoid the heating plate putting pressure on the mold and crushing the proportion during preheating). The temperature of the upper heating plate and the lower heating plate are both 580-680°C for heating, so that when the glass 3 is heated to a certain softening degree, it is pressed down to a semi-formed state by the dead weight of the arc mold 4. In addition, this positioning and local low-temperature molding method reduces poor thermal molding and mold marks, improves the yield rate and reduces the subsequent polishing time.
[0055] Step S3, after preheating is completed, the processing mold is moved to the forming station, the part of the glass 3 in the horizontal cavity is pressed down at a temperature of 400-520°C and the pressure is maintained, and the part of the glass 3 opposite to the arc cavity is slowly pressed down at a temperature of 550-650°C. The arc mold 4 is pressed down until the part of the glass 3 is attached to the lower mold 2.
[0056] Specifically, when the overall temperature of the glass 3 reaches the expected level, the glass 3 softens to a certain degree, and the molding range reaches the expected level, the processing mold is pushed into the molding station, the glass 3 in the non-molding area is continuously maintained at a temperature of 400-520°C, and pressure is applied to the glass 3 in the molding area at a temperature of 550-650°C to press the arc mold 4 downward, thereby making the glass 3 completely fit the lower mold 2 for molding.
[0057] In step S2 and / or step S3, the temperature difference between the horizontal cavity and the arc cavity is ΔT1, wherein ΔT1≤180° C. That is, the temperature difference between the forming area and the non-forming area of the glass is ≤180° C. If the temperature difference is greater than 180° C., it is easy to cause excessive stress in the glass 3 in the forming area and the non-forming area and cause cracking.
[0058] The temperature difference between the molding temperature of the part of the glass 3 opposite to the arc cavity in step S3 and the preheating temperature of the glass in step S2 is ΔT2, where 25<ΔT2<35℃. That is, the molding temperature of the molding area in step S3 is 25-35℃ lower than the preheating temperature in step S2. The high preheating temperature is because the higher softening degree can better make the glass semi-molded under the weight of the mold; the lower molding temperature is because the lower softening degree will not form a mold mark on the glass surface when the mold is pressed down, while the higher temperature and higher softening degree will form a mold mark on the glass surface when the mold is pressed down. 25-35℃ is a better temperature range. A temperature difference greater than 35℃ may cause insufficient softening during molding and thus fail to form well; a temperature difference less than 25℃ will still form a mold mark on the glass surface.
[0059] In step S2 and / or S3, the preheating temperature and / or the forming temperature of the forming area are related to the thickness and bending amplitude of the glass. The greater the thickness, the higher the required temperature. The greater the bending amplitude, the higher the required temperature. In steps S2 and S3, the temperature of the non-forming area remains unchanged.
[0060] Step S4, annealing and cooling the bent glass 3 in sequence, and then trimming the shape of the glass 3 to obtain a finished glass 3. The specific operation process is as follows:
[0061] Step S41, move the processing mold to the annealing area, and keep the processing mold under pressure at a temperature of 380-480℃ and slowly cool it down. Specifically, first push the mold into the pressure-keeping and slow-cooling area at a temperature of 300-400℃, and apply pressure to the molding area and non-molding area of the mold to prevent warping and deformation, and keep the pressure and slowly cool it down to the preset temperature. Fig. 9 As shown, when the glass 3 reaches the preset temperature, the processing mold is moved to the annealing zone, and the upper heating plate and the lower heating plate are continuously pressurized and the temperature is maintained at 300-400° C., so that the processing mold is pressurized and slowly cooled.
[0062] In step S41, the annealing temperature is lower than the preheating temperature of the non-forming area, ensuring that the glass in the non-forming area also undergoes the annealing process.
[0063] Step S42, the cooled processing mold is moved to a cooling station, so that the processing mold is cooled to room temperature, and the glass 3 is taken out to obtain a semi-finished product.
[0064] Specifically, the processing mold is pushed into the cooling zone as a whole, and the upper and lower pressing plates are in contact with the processing mold through cooling water to cool the processing mold to room temperature, and the glass 3 is taken out to obtain a semi-finished product.
[0065] Step S43, CNC precision carving removes the positioning area (groove 31 area) of the glass 3, the cutting edge is selected at the arc position, and the tangent line extending from the arc edge forms an angle of 0-10° with the edge of the glass 3 to cut the remaining material.
[0066] Specifically, after the glass 3 is taken out after molding, it is subjected to secondary fine carving, and the groove 31 area is ground and removed. The intersection of the secondary fine carving and the first fine carving is selected at the edge of the arc R angle of the product, and is finely carved by a tangent bevel processing method with an angle of 0 to 10 degrees. This can more effectively reduce the intersection marks and better ensure the contour size of the product.
[0067] Step S44, polishing the sharp corners of the edges on both sides until they are smooth to obtain the desired curved glass 3.
[0068] Specifically, the edge of the glass 3 that has been finely carved twice is polished, and the intersection of the two fine carvings is polished and smooth, so as to obtain the expected curved glass 3. The method of fine carving and polishing the glass 3 can not only ensure the contour accuracy of the glass 3, but also avoid step-shaped defects with different height differences at the intersection due to the problem of the precision of the secondary fine carving.
[0069] The following is an explanation with specific embodiments and comparative examples.
[0070] Example 1
[0071] The processing method of the curved glass with one side bent, using the above processing mold, comprises the following steps:
[0072] Step S1, the shape of the 2D glass 3 is processed by CNC precision engraving, a groove 31 reserved for positioning is processed on the non-bending side, the glass is placed in the lower mold 2, and the horizontal section of the glass 3 is limited by a limiter, the arc mold 4 is placed above the corresponding glass 3, and pressure is applied to press the horizontal mold 5 on the corresponding glass;
[0073] Step S2, sending the processing mold with the glass 3 into the heat bending machine for preheating, wherein the preheating temperature of the part of the glass 3 in the horizontal cavity is 400° C., and the preheating temperature of the part of the glass 3 opposite to the arc cavity is 580° C., so that the part of the glass 3 is softened and formed to a semi-formed state under the gravity of the arc mold 4;
[0074] Step S3, after the preheating is completed, the processing mold is moved to the forming station, the part of the glass 3 in the horizontal cavity is pressed down at a temperature of 400°C and the pressure is maintained, and the part of the glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at a temperature of 550°C until the part of the glass 3 is attached to the lower mold 2;
[0075] Step S4, annealing and cooling the bent glass 3 in sequence, and then trimming the glass shape to obtain a finished glass;
[0076] Wherein step S4 specifically comprises the following steps:
[0077] Step S41, moving the processing mold to the annealing zone, and keeping the processing mold at a temperature of 300° C. and slowly cooling it down;
[0078] Step S42, the cooled processing mold is moved to a cooling station, and cooling water is passed through the upper and lower pressing plates to contact the processing mold, so that the processing mold is cooled to room temperature, and the glass is taken out to obtain a semi-finished product;
[0079] Step S43, CNC precision carving removes the groove 31 area of the glass, the cutting edge is selected at the arc position, and the tangent line extending from the arc edge forms an angle of 0-10° with the glass edge to cut the remaining material;
[0080] Step S44, polishing the sharp corners of the edges on both sides until they are smooth to obtain the desired curved glass 3.
[0081] Example 2
[0082] The difference between this embodiment and embodiment 1 is only that:
[0083] In step S2, the preheating temperature of the portion of glass 3 in the horizontal cavity is 520°C, and the preheating temperature of the portion of glass 3 opposite to the arc cavity is 680°C;
[0084] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at a temperature of 520° C. and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at a temperature of 650° C.;
[0085] In step S41, the processing mold is maintained at a temperature of 400°C and the temperature is slowly reduced.
[0086] Example 3
[0087] The difference between this embodiment and embodiment 1 is only that:
[0088] In step S2, the preheating temperature of the portion of glass 3 in the horizontal cavity is 460°C, and the preheating temperature of the portion of glass 3 opposite to the arc cavity is 630°C;
[0089] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at a temperature of 480°C and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at a temperature of 605°C;
[0090] In step S41, the processing mold is maintained at a temperature of 350°C and the temperature is slowly reduced.
[0091] Example 4
[0092] The difference between this embodiment and embodiment 1 is only that:
[0093] In step S2, the preheating temperature of the portion of glass 3 in the horizontal cavity is 500°C, and the preheating temperature of the portion of glass 3 opposite to the arc cavity is 580°C;
[0094] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at a temperature of 520°C and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at a temperature of 555°C;
[0095] In step S41, the processing mold is maintained at a temperature of 400°C and the temperature is slowly reduced.
[0096] Comparative Example 1
[0097] The difference between this comparative example and Example 1 is only that:
[0098] In step S2, the preheating temperature of the portion of glass 3 in the horizontal cavity is 400°C, and the preheating temperature of the portion of glass 3 opposite to the arc cavity is 680°C;
[0099] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at 400°C and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at 630°C.
[0100] Comparative Example 2
[0101] The difference between this comparative example and Example 1 is only that:
[0102] In step S2, the preheating temperature of the portion of glass 3 in the horizontal cavity is 400°C, and the preheating temperature of the portion of glass 3 opposite to the arc cavity is 620°C;
[0103] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at 400°C and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at 590°C.
[0104] Comparative Example 3
[0105] The difference between this comparative example and Example 1 is only that:
[0106] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at 400°C and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at 580°C.
[0107] Comparative Example 4
[0108] The difference between this comparative example and Example 1 is only that:
[0109] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at 400°C and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at 560°C.
[0110] Comparative Example 5
[0111] The difference between this comparative example and Example 1 is only that:
[0112] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at 400°C and the pressure is maintained, and the portion of glass 3 opposite to the arc cavity is slowly pressed down on the arc mold 4 at 600°C.
[0113] Comparative Example 6
[0114] The difference between this comparative example and Example 2 is only that:
[0115] In step S2, the preheating temperature of the portion of glass 3 in the horizontal cavity is 550°C;
[0116] In step S3, the portion of glass 3 in the horizontal cavity is pressed down at a temperature of 550° C. and the pressure is maintained.
[0117] In Examples 1-4, a curved glass 3 with one side bending can be obtained by one-time molding, and the size is accurate, and there is no defect such as mold mark on the surface of the glass 3. In Comparative Examples 1-2, although the preheating temperature and molding temperature are within the range disclosed in this application, the preheating temperature difference between the molding area and the non-molding area in Comparative Example 1 is 280°C, and the molding temperature difference is 230°C; the preheating temperature difference between the molding area and the non-molding area in Comparative Example 2 is 220°C, and the molding temperature difference is 190°C. Finally, the curved glass 3 obtained in Comparative Examples 1-2 has been broken, which is due to the excessive internal stress of the glass 3 caused by the excessive temperature difference. In fact, through more tests, the probability of the curved glass 3 breaking at a temperature difference of 190-200°C is greater than 40%, the probability of the curved glass 3 breaking at a temperature difference of 200-220°C is greater than 60%, the probability of the curved glass 3 breaking at a temperature difference of more than 220°C is greater than 80%, and the curved glass 3 obtained at a temperature difference of less than 180°C will not break.
[0118] In comparative example 3, the molding temperature is equal to the preheating temperature, in comparative example 4, the molding temperature is 20°C lower than the preheating temperature, and in comparative example 5, the molding temperature is higher than the preheating temperature. Mold marks appear on the curved surfaces of the curved glass 3 obtained in comparative examples 3-5. Excessive surface molding temperature will cause mold marks to form on the surface of the glass 3. The difference is that the mold marks of comparative examples 3 and 5 are deep, and the mold marks of comparative example 4 are shallow. It is proved through experiments that the temperature difference of 25-25°C has a better molding effect and will not form mold marks on the surface of the glass 3.
[0119] In Comparative Example 6, the temperature of the non-forming area is 550°C, and the curved glass 3 obtained due to the excessively high temperature forms mold marks and concave-convex spots on the surface of the flat part; experiments have shown that when the preheating temperature and the forming temperature of the non-forming area are 400-520°C, the glass 3 can be made harder without defects such as mold marks and concave-convex spots. When the temperature is greater than 520°C, there is a high probability that mold marks and concave-convex spots will appear.
[0120] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0121] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments described herein, but should conform to the widest scope consistent with the principles and novel features invented herein.
Claims
1. A method for processing curved glass with one side bent, characterized in that: The processing method comprises the following steps: Step S1, placing the glass (3) into the lower mold (2), and limiting the horizontal section of the glass (3) by means of a limiting member, and then placing the horizontal mold (5) and the arc mold (4) above the glass (3) respectively; Step S2, sending the processing mold containing the glass (3) into the heat bending machine for preheating, wherein the preheating temperature of the part of the glass (3) in the horizontal cavity is 400-520° C., and the preheating temperature of the part of the glass (3) opposite to the arc cavity is 580-680° C., so that the part of the glass (3) is softened and formed to a semi-formed state under the gravity of the arc mold (4); Step S3, after the preheating is completed, the processing mold is moved to the forming station, the part of the glass (3) in the horizontal cavity is pressed down at a temperature of 400-520° C. and the pressure is maintained, and the part of the glass (3) opposite to the arc cavity is slowly pressed down on the arc mold (4) at a temperature of 550-650° C. until the part of the glass (3) is attached to the lower mold (2); Step S4, annealing and cooling the bent glass (3) in sequence, and then trimming the shape of the glass (3) to obtain a finished glass (3); In step S2 and / or step S3, the temperature difference between the horizontal cavity and the arc cavity is ΔT1, wherein ΔT1≤180° C.; The temperature difference between the forming temperature of the portion of glass (3) opposite to the arc-shaped cavity in the step S3 and the preheating temperature in the step S2 is ΔT2, wherein 25<ΔT2<35°C.
2. The method for processing single-side curved glass according to claim 1, characterized in that: The step S4 further comprises the following steps: Step S41, moving the processing mold to the annealing zone, and keeping the processing mold at a temperature of 300-400° C. and slowly cooling it down; Step S42, the cooled processing mold is moved to a cooling station, so that the processing mold is cooled to room temperature, and the glass (3) is taken out to obtain a semi-finished product; Step S43, fine carving to remove the positioning area of the glass (3), the cutting edge is selected at the arc position, and the tangent line is extended from the arc edge to form an angle of 0-10° with the edge of the glass (3) to cut the remaining material; Step S44, polishing the sharp corners of the edges on both sides until they are smooth to obtain the desired curved glass (3).
3. A processing mold for realizing the processing method of single-side curved glass as claimed in claim 1 or 2, characterized in that: The processing mold comprises an upper mold (1) and a lower mold (2) which are interlocked with each other, a molding cavity matching the shape of the single-sided curved glass (3) to be molded is formed between the upper mold (1) and the lower mold (2), the molding cavity comprising an arc cavity and a horizontal cavity, the upper mold (1) comprising an arc mold (4) arranged opposite to the arc cavity and a horizontal mold (5) arranged opposite to the horizontal cavity, and a limiting member is provided in the horizontal cavity for limiting the position of the horizontal section of the single-sided curved glass (3) in the horizontal direction.
4. The processing mold for curved glass with one side bent according to claim 3, characterized in that: A groove (31) is provided on the horizontal section of the single-sided curved glass (3), and the limiting member comprises a limiting block (21) arranged on the lower mold (2) and used for being inserted into the groove (31).
5. The processing mold for curved glass with one side bent according to claim 4, characterized in that: A portion of the limit block (21) extends out of the slot (31), and the limit member further comprises a limit slot (51) arranged on the horizontal mold (5) into which the extended end of the limit block (21) can be inserted.
6. The processing mold for curved glass with one side bent according to claim 5, characterized in that: The lower mold (2) comprises a bottom shell (22) and a bottom mold (23) arranged inside the bottom shell (22); the top surface of the bottom mold (23) is formed with a lower support surface matching the shape of the single-sided curved glass (3) to be formed; the top of the lower support surface is located below the top of the bottom shell (22).
7. The processing mold for curved glass with one side bent according to claim 6, characterized in that: The horizontal mold (5) comprises a first cover plate (52) and a horizontal mold body (53) arranged on the side of the first cover plate (52), and the horizontal cavity is formed between the horizontal mold body (53) and the horizontal section of the bottom mold (23).
8. The processing mold for curved glass with one side bent according to claim 7, characterized in that: Insertion plates (54) are provided on both sides of the first cover plate (52), slots (24) matching the insertion plates (54) are provided on both sides of the bottom shell (22), a first guide plate (55) is provided on the inner side of the insertion plate (54), and a first guide groove (25) matching the first guide plate (55) is provided on the bottom shell (22).
9. The processing mold for curved glass with one side bent according to claim 6, characterized in that: The arc-shaped mold (4) comprises a second cover plate (41) and an arc-shaped mold body (42) arranged on the side of the second cover plate (41), and the arc-shaped cavity is formed between the arc-shaped mold body (42) and the arc-shaped segment of the bottom mold (23).
10. The processing mold for curved glass with one side bent according to claim 9, characterized in that: Second guide plates (43) are respectively provided on both sides of the arc-shaped mold body (42), and second guide grooves (26) matching the second guide plates (43) are provided on the bottom shell (22).
Citation Information
Patent Citations
Curved-glass hot-bending mould and hot-bending process thereof
CN107572762A
Concave panel and forming method thereof
CN108019798A
Unilateral hot -bend forming mould of curved product of heat
CN206375818U
Local curved glass processing mold and curved glass hot bending machine
CN217628112U
Positive pressure-supported gravity bending method and device suitable for said method
WO2017089070A1