A kind of ampere-level high current density electrocatalytic hydrogen evolution catalyst and preparation method
The preparation of platinum-rare earth bimetallic single atoms and alloy clusters supported by the hollow carbon-based support through ion exchange and closed space calcination strategies was solved, and the problem of poor stability of platinum-based catalysts and nanoparticle agglomeration under large current density was solved, and the problem of nanoparticle agglomeration was achieved. A catalyst with high activity, low load and strong durability, suitable for industrial electrolytic hydrogen production technology.
Patent Information
- Application Number
- CN202211262731.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-10-14
AI Technical Summary
Existing platinum-based catalysts are difficult to operate stably under high current density. The high surface free energy of precious metals leads to easy agglomeration of metals, and the nanoparticle size is controlled by surfactants during the synthesis process, resulting in low platinum utilization.
Using ion exchange and closed space calcination strategies, the composite materials with platinum-rare earth bimetallic monomer and alloy clusters supported by hollow carbon-based support are prepared, which avoids the use of surfactants, and introduces rare earth ions through ion exchange and forms at low temperature heat treatment. Oxidation of rare earth/silica precursors, followed by pyrolytic carbonization to remove the silica template, forming Pt, Re metal single atoms and PtRe alloy cluster catalysts supported on hollow carbon substrates.
It has achieved stable operation for 1000 hours at a high current density of 1.0A/cm2, maintaining high Pt exposure and utilization rate, overcomes the problems of surfactant residue and nanoparticle agglomeration, is low-cost and universal, and is suitable for industrial production. .
Smart Images

Figure CN115786930B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of alloy cluster and metal single atom catalyst preparation, and relates to an ampere-level high current density electrocatalytic hydrogen evolution catalyst and a preparation method, and specifically relates to an ion exchange and closed space confinement method for preparing a composite material of platinum-rare earth bimetallic single atoms and alloy clusters loaded on a hollow carbon-based carrier, wherein the alloy clusters on the surface exhibit a platinum-rich surface. Background Art
[0002] As the cleanest and most efficient energy source, the large-scale production of hydrogen is conducive to alleviating the energy crisis and environmental problems. As one of the most promising preparation technologies, hydrogen production by water electrolysis has attracted widespread attention. Among them, platinum is considered to be the most effective catalyst for hydrogen production by water electrolysis. However, the scarcity, high cost and poor stability of precious metals are the key factors restricting the widespread commercial deployment of this technology. In addition, rare earth elements are widely used in metallurgy, electronics and catalysis due to their unique electronic, optical and magnetic properties. Compared with single metal catalysts, the charge transfer between two different surface atoms in alloy catalysts will change the electronic structure of Pt and the adsorption energy of reaction intermediates. At the same time, reducing the catalyst size to the cluster or even single atom level is conducive to significantly improving the catalytic activity of Pt, which is conducive to improving the atomic utilization while maintaining or even reducing the use of precious metals, thereby reducing costs.
[0003] Hollow structure carriers are conducive to increasing the loading sites of active species, thereby increasing the contact area with reactants and the number of effective active sites. At the same time, the introduction of nitrogen elements is also conducive to the stability of active centers.
[0004] In addition, the synthesis process of small-sized alloy catalysts usually inevitably uses surfactants that are difficult to remove, resulting in the burial of active sites, which seriously reduces the utilization rate of platinum. At the same time, the problem of nanoparticles easily agglomerating at high temperatures also needs to be solved. Most importantly, stable catalytic production of hydrogen at high current density is still a huge challenge for platinum-based catalysts. Summary of the invention
[0005] Technical issues to be solved
[0006] In order to avoid the shortcomings of the prior art, the present invention proposes an ampere-level high current density electrocatalytic hydrogen evolution catalyst and a preparation method. In view of the current technical status that platinum-based catalysts are difficult to work stably at high current densities, and the high surface free energy of precious metals makes metals easy to agglomerate and inevitably relies on surfactants to control the size of alloy nanoparticles during the synthesis process, an ion exchange combined with a closed space calcination strategy is provided to prepare bimetallic single atoms and alloy clusters distributed on a hollow carbon-based carrier, wherein the alloy clusters exhibit an alloy structure with a Pt-rich surface. The prepared catalyst is an industrial water electrolysis catalyst that can work stably at ampere-level high current densities. The method enables the prepared catalyst to have the characteristics of low load, high activity and strong durability. At the same time, the method can cover the preparation of catalysts for Pt-based bimetallic single atoms and alloy clusters loaded on various carbon-based carriers.
[0007] Technical Solution
[0008] An ampere-level high current density electrocatalytic hydrogen evolution catalyst, characterized in that the catalyst uses a hollow carbon base as a carrier, bimetallic single atoms and alloy clusters are loaded on the hollow carbon base carrier, and the alloy clusters on the surface show a platinum-rich surface. The ampere-level high current density is not less than 1.0A / cm 2 .
[0009] The types of the bimetallic single atoms include a combination of Pt and La, Ce, Sm, Eu, Gd, Pr or Er.
[0010] The types of the surface alloy clusters correspond to PtLa, PtCe, PtSm, PtEu, PtGd, PtPr or PtEr respectively.
[0011] A method for preparing the ampere-level high current density electrocatalytic hydrogen evolution catalyst, characterized by the following steps:
[0012] Step 1, preparation of precursor: placing silica microspheres containing rare earth metal ions in a muffle furnace, heating the temperature to 200-400° C. at 10° C. / min, and then maintaining the temperature for 0.5-5 h to obtain a silica / metal oxide precursor;
[0013] Step 2: Ultrasonic dispersion of silica / metal oxide precursor in a mixed solution of deionized water and ethanol, and adding a mixed solution containing a noble metal Pt source, and adding a mixed solution containing ammonia water after immersion reaction at room temperature for 2-12 hours, stirring for 0.5-3 hours, and then adding a mixed solution of water and ethanol containing dopamine hydrochloride, and continuing to stir and react at room temperature for 12 hours;
[0014] The noble metal Pt source is chloroplatinic acid;
[0015] Step 3: After the reaction is completed, the product is centrifuged, washed with water and ethanol, separated, dried, and then transferred to a tubular furnace under a nitrogen atmosphere and heated to 600-900°C at a rate of 5°C / min for calcination for 2 hours. The calcined product is placed in an aqueous solution of ammonium bifluoride and reacted at 80°C for 2-6 hours to remove the silica template, thereby obtaining a hollow carbon-based carrier loaded with bimetallic single atoms and alloy cluster materials, i.e., an ampere-level high current density electrocatalytic hydrogen evolution catalyst.
[0016] The preparation of the silica microspheres containing rare earth metal ions comprises: ultrasonically dispersing silica microspheres rich in ammonium ions into deionized water, adding rare earth metal salts for 20 minutes, stirring at 80° C. for ion exchange reaction for 12-18 hours; then centrifuging, separating, washing, and drying to obtain silica microspheres containing rare earth metal ions.
[0017] The rare earth metal salt is a nitrate of La, Ce, Sm, Eu, Gd, Pr or Er.
[0018] The types of silica / metal oxide precursors correspond to silica / La, Ce, Sm, Eu, Gd, Pr or Er oxides, respectively.
[0019] The concentration of the silica microspheres is 0.58 mol / L.
[0020] The rare earth metal salt concentration range is 3.13 mmol / L-50.00 mmol / L.
[0021] The water and ethanol in step 2 V 水 :V 乙醇 =1:1.
[0022] Beneficial Effects
[0023] The present invention provides an ampere-level high current density electrocatalytic hydrogen evolution catalyst and a preparation method thereof. Firstly, rare earth ions (Re n+ =Er 3+ ,La 3+ 、Ce 3+ 、Sm 3+ 、Eu 3+ , Gd 3+ , Pr 3+The present invention is to prepare a catalyst for the synthesis of rare earth oxide / silicon dioxide. The precursor is introduced into the composite precursor of rare earth oxide / silicon dioxide by heat treatment at low temperature in air. The precursor is introduced into the precious metal Pt source while coating the polymer shell. Finally, the silica template is removed after pyrolysis and carbonization to obtain a catalyst of Pt, Re metal single atoms and PtRe alloy clusters supported on a hollow carbon-based carrier. The prepared catalyst is supported by a hollow carbon-based carrier, and metal Pt, Re single atoms and PtRe alloy clusters are distributed on the surface of the carbon-based carrier, wherein the PtRe alloy clusters show an alloy structure with a rich Pt surface. Compared with the prior art, the ion exchange used in the present invention ensures the diversity of non-precious metals in the precursor, and the PtRe alloy clusters formed on the rich Pt surface improve the stability of the alloy structure while maintaining high Pt exposure and utilization. The elastic space created between silica and polymer is conducive to the alloying process and particle size restriction, while avoiding the use of surfactants to bury the active sites, overcoming the problems of poor adhesion of traditional wet chemical impregnation, particle agglomeration during high temperature treatment, and easy dealloying during catalysis. In addition, this method is simple in process, can be synthesized in large quantities and has universal applicability, and is suitable for the preparation of a variety of precious metal-rare earth metal combined nano alloy clusters and single atom catalysts. The catalyst is used for high current density (≥1.0A / cm 2 ) for more than 1000 hours under continuous water electrolysis, with excellent results, far superior to commercial Pt / C (20wt%) catalyst, which is of great significance to promoting the development of industrial-grade water electrolysis hydrogen production technology.
[0024] The beneficial effects of the present invention are:
[0025] 1. The present invention adopts ion exchange and closed space calcination strategy. No surfactant is required in the alloy preparation process. The synthesized nanoframe alloy is small in size and evenly distributed, which not only ensures the diversity of precursors, but also overcomes the problems of surfactant residue shielding the active sites and high-temperature agglomeration of nanoparticles. It has excellent electrochemical performance and can be used at 1.0A / cm 2 It can run stably for 1000 hours at the above high current density with almost no activity decay.
[0026] 2. This method is universal and applicable to the preparation of a variety of single atom-alloy cluster hybrids loaded on hollow carbon-nitrogen carrier materials.
[0027] 3. The process of the present invention is simple and safe, low-cost, and has the advantages of controllable preparation and large-scale synthesis, and is suitable for industrial production and large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 TEM image of the precursor prepared in Example 1
[0029] Figure 2 TEM image of the platinum-erbium bimetallic single atoms and alloy clusters prepared in Example 1 supported on a hollow carbon-based carrier catalyst
[0030] Figure 3 Spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscopy image of the platinum-erbium bimetallic single atoms and alloy clusters supported on the hollow carbon-based carrier catalyst prepared in Example 1
[0031] Figure 4 The platinum-erbium bimetallic single atoms and alloy clusters prepared in Example 1 were loaded on a hollow carbon-based carrier catalyst at 1.0 A / cm 2 Stability curve under high current density
[0032] Figure 5 TEM image of the platinum-lanthanum bimetallic single atoms and alloy clusters prepared in Example 2 supported on a hollow carbon-based carrier catalyst DETAILED DESCRIPTION
[0033] The present invention will now be further described with reference to the embodiments and the accompanying drawings:
[0034] The technical solution of the present invention is as follows:
[0035] A method for preparing an ampere-level high current density electrocatalytic hydrogen evolution catalyst, characterized in that the method comprises the following steps:
[0036] 1) Dispersing silica microspheres and rare earth metal salts in deionized water for cation exchange reaction, and calcining the obtained product to obtain a silica / rare earth metal oxide precursor.
[0037] 2) The precursor is dispersed in the mixed solution by ultrasonic dispersion, and the mixed solution containing the precious metal source is added at the same time. After a certain period of immersion reaction at room temperature, a mixed solution containing ammonia water is added, and then a mixed solution of water and ethanol containing dopamine hydrochloride is added for polymerization. After the reaction is completed, the product is centrifuged, washed with water and ethanol, separated, dried, and then heat-treated in a nitrogen atmosphere and the template is finally removed to obtain a material of Pt-based bimetallic single atoms and platinum-based alloy clusters loaded on a hollow carbon-based carrier.
[0038] The Pt-based bimetallic single atoms and alloy clusters prepared by the present invention are loaded on a hollow carbon-based carrier material and have excellent electrocatalytic hydrogen evolution performance, and can be used in the fields of electrocatalysis and the like. Specific embodiment:
[0040] The present invention provides a catalyst with universal single-atom and cluster alloy hybrid distribution, which uses silica microspheres as templates and inner confinement barriers, forms metal oxides in the templates through cation exchange and calcination, polydopamine seals the precious metal source and serves as an outer confinement barrier, and synchronous pyrolysis is performed to achieve alloying, and finally the template is removed to obtain a catalyst in which Pt-based bimetallic single atoms and alloy clusters are loaded on a hollow carbon-based carrier. The preparation method thereof mainly comprises the following steps:
[0041] Example 1
[0042] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 0.25 mmol of erbium nitrate and ultrasonically disperse for 20 min, then react at 80 ° C with stirring for 16 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The resulting product is calcined at 200 ° C for 4 h in an air atmosphere to obtain a precursor.
[0043] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0193 mmol of chloroplatinic acid is added, and after stirring for 6 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and 0.75 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 900 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 2 hours to remove the template, and platinum erbium single atoms and alloy clusters are loaded on hollow carbon nitrogen carrier materials.
[0044] Example 2
[0045] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 0.25 mmol of lanthanum nitrate and ultrasonically disperse for 20 min, then stir the reaction at 80 ° C for 18 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The product is calcined at 250 ° C for 5 h in an air atmosphere to obtain a precursor.
[0046] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0386 mmol of chloroplatinic acid is added, and after stirring for 5 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and after 0.5 hours, 0.75 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 900 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 2 hours to remove the template, and the platinum lanthanum single atom and alloy clusters are loaded on the hollow carbon nitrogen carrier material.
[0047] Example 3
[0048] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 1 mmol of cerium nitrate and ultrasonically disperse for 20 min, then react with stirring at 80 ° C for 18 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The obtained product is calcined at 400 ° C for 0.5 h in an air atmosphere to obtain a precursor.
[0049] Step 2: Disperse the precursor in a solution containing 20 mL of water and 20 mL of ethanol, add 10 mL of a 1:1 mixed solution of water and ethanol containing 0.0193 mmol of chloroplatinic acid, stir and react for 6 hours, add 8 mL of a 1:1 mixed solution of water and ethanol containing 2 mL of ammonia water, and stir and react for 12 hours after 3 hours. After the reaction, place the product in a tubular furnace and heat it to 800 ° C at a rate of 5 ° C / min under a nitrogen atmosphere for 2 hours. Finally, place the calcined product in a 0.09 mol NH4HF2 aqueous solution for 3 hours to remove the template, and obtain platinum cerium single atoms and alloy clusters loaded on hollow carbon nitrogen carrier materials.
[0050] Example 4
[0051] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 1 mmol of europium nitrate and ultrasonically disperse for 20 min, then react with stirring at 80 ° C for 12 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The obtained product is calcined at 400 ° C for 0.5 h in an air atmosphere to obtain a precursor.
[0052] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0193 mmol of chloroplatinic acid is added, and after stirring for 2 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and after 3 hours, 0.75 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 800 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 2 hours to remove the template, and platinum europium single atoms and alloy clusters are loaded on hollow carbon nitrogen carrier materials.
[0053] Example 5
[0054] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 0.25 mmol of praseodymium nitrate and ultrasonically disperse for 20 min, then react with stirring at 80 ° C for 16 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The obtained product is calcined at 200 ° C for 4 h in an air atmosphere to obtain a precursor.
[0055] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0193 mmol of chloroplatinic acid is added, and after stirring for 4 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and 0.75 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 900 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 3 hours to remove the template, and the platinum praseodymium single atom and alloy clusters are loaded on the hollow carbon nitrogen carrier material.
[0056] Example 6
[0057] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 0.25 mmol of samarium nitrate and ultrasonically disperse for 20 min, then react with stirring at 80 ° C for 16 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The obtained product is calcined at 200 ° C for 4 h in an air atmosphere to obtain a precursor.
[0058] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0193 mmol of chloroplatinic acid is added, and after stirring for 6 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and 0.9 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 900 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 2 hours to remove the template, and the platinum samarium single atom and alloy clusters are loaded on the hollow carbon nitrogen carrier material.
[0059] Example 7
[0060] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 1 mmol of gadolinium nitrate and ultrasonically disperse for 20 min, then stir and react at 80° C. for 12 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The resulting product is calcined at 200° C. for 4 h in an air atmosphere to obtain a precursor.
[0061] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0193 mmol of chloroplatinic acid is added, and after stirring for 6 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and 0.75 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 900 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 2 hours to remove the template, and platinum gadolinium single atoms and alloy clusters are loaded on the hollow carbon nitrogen carrier material.
[0062] Example 8
[0063] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 0.125 mmol of erbium nitrate and ultrasonically disperse for 20 min, then react at 80 ° C with stirring for 16 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The product is calcined at 250 ° C for 5 h in an air atmosphere to obtain a precursor.
[0064] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0097 mmol of chloroplatinic acid is added, and after stirring for 12 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and 0.9 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 600 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 2 hours to remove the template, and platinum erbium single atoms and alloy clusters are loaded on the hollow carbon nitrogen carrier material.
[0065] Example 9
[0066] Step 1: Disperse 500 mg of silica microspheres in 40 mL of water, add 2 mmol of erbium cobalt nitrate and ultrasonically disperse for 20 min, then react with stirring at 80 ° C for 18 h. After the reaction is completed, centrifuge, separate, and vacuum dry. The obtained product is calcined at 400 ° C for 0.5 h in an air atmosphere to obtain a precursor.
[0067] Step 2: The precursor is dispersed in a solution containing 20 mL of water and 20 mL of ethanol, and 10 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 0.0386 mmol of chloroplatinic acid is added, and after stirring for 5 hours, 8 mL of a mixed solution of water and ethanol with a volume ratio of 1:1 containing 2 mL of ammonia water is added, and 1 hour later, 1.2 mmol of dopamine is weighed and dissolved in 30 mL of a mixed solution of water and ethanol with a volume ratio of 1:1, and then stirred for 12 hours. After the reaction is completed, the product is placed in a tubular furnace under a nitrogen atmosphere and heated to 900 ° C at a rate of 5 ° C / min for 2 hours. Finally, the calcined product is placed in a 0.09 mol NH4HF2 aqueous solution for 6 hours to remove the template, and platinum erbium single atoms and alloy clusters are loaded on the hollow carbon nitrogen carrier material.
[0068] Table 1 shows the atomic ratio of Pt and Er elements obtained by X-ray photoelectron spectroscopy of platinum-erbium bimetallic single atoms and alloy clusters loaded on hollow carbon-based carrier catalysts prepared in Example 1, which is higher than the value obtained by inductively coupled plasma mass spectrometry, proving the successful preparation of PtEr alloy clusters with Pt-rich surfaces.
[0069] Pt / Er atomic ratio X-ray Photoelectron Spectroscopy 2.19 Inductively Coupled Plasma Spectroscopy 0.85
Claims
1. An ampere-level high current density electrocatalytic hydrogen evolution catalyst, characterized in that The catalyst is supported by a hollow carbon base, and the bimetallic single atoms and alloy clusters are loaded on the hollow carbon base. The alloy clusters on the surface show a platinum-rich surface. The ampere-level large current density is not less than 1.0 A / cm 2 ; The type of the bimetallic single atom is a combination of Pt and La, Ce, Sm, Eu, Gd, Pr or Er; The types of the surface alloy clusters correspond to PtLa, PtCe, PtSm, PtEu, PtGd, PtPr or PtEr respectively; The method for electrocatalyzing hydrogen evolution with an ampere-level high current density comprises the following steps: Step 1, preparation of precursor: placing silica microspheres containing rare earth metal ions in a muffle furnace, heating the temperature to 200-400°C at 10°C / min, and then keeping the temperature constant for 0.5-5 h to obtain a silica / metal oxide precursor; Step 2: Ultrasonic dispersion of silica / metal oxide precursor in a mixed solution of deionized water and ethanol, and adding a mixed solution containing a noble metal Pt source, and adding a mixed solution containing ammonia water after immersion reaction at room temperature for 2-12 hours, stirring for 0.5-3 hours, and then adding a mixed solution of water and ethanol containing dopamine hydrochloride, and continuing to stir and react at room temperature for 12 hours; The noble metal Pt source is chloroplatinic acid; Step 3: After the reaction is completed, the product is centrifuged, washed with water and ethanol, separated, dried, and then transferred to a tubular furnace and heated to 600-900 °C at a rate of 5 °C / min for 2 h in a nitrogen atmosphere for calcination. The calcined product is placed in an aqueous solution of ammonium bifluoride and reacted at 80 °C for 2-6 h to remove the silica template, thereby obtaining a hollow carbon-based carrier loaded with bimetallic single atoms and alloy cluster materials, i.e., an ampere-level high current density electrocatalytic hydrogen evolution catalyst; Preparation of the silica microspheres containing rare earth metal ions: ultrasonically disperse silica microspheres rich in ammonium ions in deionized water, add rare earth metal salts for 20 minutes, stir at 80°C for ion exchange reaction for 12-18 hours; then centrifuge, separate, wash, and dry to obtain silica microspheres containing rare earth metal ions; The concentration of the silica microspheres is 0.58 mol / L, and the concentration range of the rare earth metal salt is 3.13 mmol / L-50.00 mmol / L.
2. The ampere-level high current density electrocatalytic hydrogen evolution catalyst according to claim 1, characterized in that: The rare earth metal salt is a nitrate of La, Ce, Sm, Eu, Gd, Pr or Er.
3. The ampere-level high current density electrocatalytic hydrogen evolution catalyst according to claim 1, characterized in that: The types of silica / metal oxide precursors correspond to silica / oxides of La, Ce, Sm, Eu, Gd, Pr or Er, respectively.
4. The ampere-level high current density electrocatalytic hydrogen evolution catalyst according to claim 1, characterized in that: The water and ethanol in step 2 V 水 : V 乙醇 = 1:1.