Fabric with radiation cooling and photoelectric heat conversion functions and preparation method thereof

By fixing carbon nanomaterials on the front of the fabric and spraying ZnO@ZIF-8@SiO2 layer on the back, combined with the hydrophobic treatment of PDMS, the temperature regulation and self-cleaning effect of rapid response in extreme temperature environments is achieved, and the existing solution is solved The technology cannot adapt to the problem of heating in cold weather and is suitable for multifunctional textiles.

CN115787294BActive Publication Date: 2024-11-26ANHUI LINNENG TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211585808.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-26
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Existing radiation cooling materials cannot be effectively heated in cold weather, resulting in the inability to adapt to temperature fluctuations in extreme temperature environments, the inability to quickly respond to heating or cooling, and the difficulty in switching between hot and cold.

Method used

A fabric preparation method is adopted to achieve photoelectric and thermal conversion function by fixing carbon nanomaterials on the front of the fabric, and spraying ZnO@ZIF-8@SiO2 layer on the back to achieve radiation cooling performance, while introducing PDMS on the surface of the fabric to improve hydrophobicity to achieve self-cleaning effect.

Benefits of technology

The fabric can quickly adjust temperature in extreme temperature environments, maintain the comfortable temperature range of the human body, and has excellent self-cleaning performance, suitable for personal protection and smart materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115787294B_ABST
    Figure CN115787294B_ABST
Patent Text Reader

Abstract

The invention discloses a fabric with radiation cooling and photoelectric heat conversion functions and a preparation method thereof, comprising the following steps: 1. dipping a fabric substrate in a dopamine hydrochloride solution, washing and drying to obtain a fabric modified with dopamine hydrochloride; 2. fixing a carbon nano material on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying to obtain a fabric with a photoelectric heat conversion function; 3. weighing a PDMS prepolymer and a PDMS curing agent, dissolving them in tetrahydrofuran, and dispersing to obtain a PDMS solution; 4. dipping the fabric with the photoelectric heat conversion function in the PDMS solution, and curing to obtain a CNT / PDMS treated fabric; 5. taking nano ZnO@ZIF‑8@SiO2, an adhesive and deionized water, and then dispersing the ZnO@ZIF‑8@SiO2 and the adhesive in the deionized water to obtain a mixed solution; 6. spraying the mixed solution on the reverse side of the CNT / PDMS treated fabric, and drying to obtain a fabric with radiation cooling and photoelectric heat conversion functions, and having excellent self-cleaning performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional fabrics, and in particular relates to a fabric with radiation cooling and photoelectric heat conversion functions and a preparation method thereof. Background Art

[0002] As climate change changes, there will be more intense and frequent heat waves or cold weather, which will affect our health. When exposed to hot or cold environments, the human body feels uncomfortable due to the stress of heat or cold, causing the skin and body temperature to rise or fall. Indoor thermal comfort is generally achieved through air conditioning and fans, but in open outdoor environments, the use of air conditioning and fans is uneconomical and impractical. In order to reduce the damage to the human body caused by extreme heat or cold in outdoor spaces, local cooling or heating of the human body is required through personal thermal management. Globally, functional textiles or wearable materials involved in new personal thermal management have been used to improve the thermal comfort of the human body, and they are very popular because they are very energy-efficient.

[0003] Radiative heat management has been shown to be an effective method for personal cooling, including infrared transparent radiative cooling, infrared emitting radiative cooling, and solar reflecting radiative cooling. However, many passive radiative cooling materials can only provide cooling when the weather is warm, which often cannot adapt to temperature fluctuations in hot and cold seasons. When the temperature is lower than expected in cold weather, this radiative cooling will lead to unnecessary temperature drops and increase energy consumption caused by heating in cold weather. It can be seen that how to design a single textile that can switch between cooling and heating to adapt to various situations is still a huge challenge. In other words, there is an urgent need for a textile-based electric heating material that can heat or cool on demand, has fast response, high conversion efficiency, and a wide temperature range to adapt to seasonal temperature fluctuations in hot and cold weather. Multifunctional textiles. Summary of the invention

[0004] The purpose of the present invention is to provide a fabric with radiation cooling and photoelectric thermal conversion functions and a preparation method thereof. The front side of the fabric has the photoelectric thermal conversion function, the back side has the performance of radiation cooling, and both sides of the fabric have excellent self-cleaning performance.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a fabric having radiation cooling and photoelectric heat conversion functions comprises the following steps:

[0007] Step 1, first rinse and dry the fabric substrate, then immerse it in a dopamine hydrochloride solution, take it out, wash it and dry it to obtain a fabric modified with dopamine hydrochloride;

[0008] Step 2, dispersing the carbon nanomaterial in an organic solvent according to a ratio (0.1-0.5 g): 1 L, and then fixing the carbon nanomaterial on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying to obtain a fabric with photoelectric thermal conversion function;

[0009] Step 3, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and PDMS curing agent in tetrahydrofuran, and fully dispersing them at room temperature until a uniform and transparent PDMS solution is formed;

[0010] Step 4, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and obtaining a CNT / PDMS-treated fabric after curing;

[0011] Step 5, taking nano ZnO@ZIF-8@SiO2, a binder and deionized water in a mass ratio of (1-3):8:(1-3), and then dispersing the ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution;

[0012] Step 6: spray the mixed solution on the reverse side of the CNT / PDMS treated fabric, and after drying, obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0013] Furthermore, the rinsing in step 1 uses deionized water and anhydrous ethanol to rinse the fabric substrate alternately.

[0014] Furthermore, the fabric base in step 1 is pure cotton fabric.

[0015] Furthermore, in step 1, the concentration of dopamine hydrochloride solution is (8-10) mmol / mL, the pH value is 8.5, and the immersion time is 12-24 hours.

[0016] Furthermore, the carbon nanomaterial in step 2 is one of single-walled carbon nanotubes, multi-walled carbon nanotubes, MXene, graphene, graphene oxide or carbon black.

[0017] Furthermore, the organic solvent in step 2 is N,N-dimethylformamide, isopropanol or anhydrous ethanol.

[0018] Furthermore, the adhesive in step 5 is methacrylate or cyanoacrylate.

[0019] Furthermore, the drying temperatures of step 1, step 2 and step 6 and the curing temperature of step 4 are all 60-130°C.

[0020] A fabric with radiation cooling and photoelectric heat conversion functions.

[0021] The present invention has the following beneficial effects:

[0022] First, the present invention fixes carbon nanomaterials on the front side of the fabric as a conductive layer, giving the fabric excellent electrical properties and excellent electrothermal conversion performance; secondly, PDMS is introduced into the surface of the fabric substrate, so that the fabric exhibits excellent hydrophobicity, so that the surface is not easily contaminated with pollutants and has good self-cleaning performance; thirdly, the back side of the fabric prepared by the present invention has the performance of radiation cooling, while the front side has the characteristics of solar heating and electric heating. When the weather is too cold or too hot, the excellent cooling or heating performance of the fabric keeps the temperature of the human body in a comfortable temperature range. Finally, the method of the present invention is simple and easy to mass produce. The prepared fabric with radiation cooling, photothermal and electrothermal conversion and self-cleaning functions has broad application prospects in the fields of personal protection, smart materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 : Water contact angle of the fabric prepared in Example 3 of the present invention;

[0024] Figure 2 : Reflectivity curve of the back side of the fabric prepared in Example 3 of the present invention to the sunlight band;

[0025] Figure 3 : Absorption rate curve of the fabric prepared in Example 3 of the present invention facing the sunlight band;

[0026] Figure 4 : Temperature test characterization comparison diagram of the fabric prepared in Example 3 of the present invention and ordinary fabric. DETAILED DESCRIPTION

[0027] The specific contents of the present invention are further explained in detail below in conjunction with the embodiments, but are not intended to limit the present invention.

[0028] The ZnO@ZIF-8@SiO2 used in the present invention is prepared according to the methods described in the following documents [1] and [2]:

[0029] [1]Keep Cool:Polyhedral ZnO@ZIF-8Polymer Coatings for DaytimeRadiative Cooling[J]. Industrial And Engineering Chemistry Research, 2020, 59(34):15226-15232.

[0030] [2] Fan Yuanrui, Zhang Wei, Chen Yuantao, et al. Preparation of ZIF-8-SiO2 and its adsorption of U(VI)[J]. Journal of Composite Materials, 2021, 38(9): 3064-3072.

[0031] Example 1

[0032] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 60°C to obtain a clean fabric base;

[0033] Step 2, placing a clean fabric substrate into a dopamine hydrochloride solution with a concentration of 10 mmol / mL and a pH value of 8.5, immersing for 12 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 60° C. to obtain a fabric modified with dopamine hydrochloride;

[0034] Step 3, ultrasonically dispersing the multi-walled carbon nanotubes in N,N-dimethylformamide at a ratio of 0.1 g:1 L to obtain solution A;

[0035] Step 4, fixing the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and then drying in an oven at 60° C. to obtain a fabric with photoelectric thermal conversion function;

[0036] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and the PDMS curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0037] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 60° C. to obtain a CNT / PDMS-treated fabric;

[0038] Step 7, taking nano ZnO@ZIF-8@SiO2, a binder and deionized water in a mass ratio of 1:8:1, ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and methacrylate in deionized water to obtain a mixed solution B;

[0039] Step 8: spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 120° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0040] Example 2

[0041] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 100°C to obtain a clean fabric base;

[0042] Step 2, placing a clean fabric substrate in a dopamine hydrochloride solution with a concentration of 8 mmol / mL and a pH value of 8.5, immersing for 16 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 100° C. to obtain a fabric modified with dopamine hydrochloride;

[0043] Step 3, ultrasonically disperse MXene in isopropanol at a ratio of 0.2 g: 1 L to obtain solution A;

[0044] Step 4: Fix the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and then dry it in an oven at 100° C. to obtain a fabric with photoelectric thermal conversion function;

[0045] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and the PDMS curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0046] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 100° C. to obtain a CNT / PDMS-treated fabric;

[0047] Step 7, taking nano ZnO@ZIF-8@SiO2, a binder and deionized water in a mass ratio of 2:8:2, ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and methacrylate in deionized water to obtain a mixed solution B;

[0048] Step 8: spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 100° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0049] Example 3

[0050] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 80°C to obtain a clean fabric base;

[0051] Step 2, placing a clean fabric substrate into a dopamine hydrochloride solution with a concentration of 10 mmol / mL and a pH value of 8.5, immersing for 20 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 80° C. to obtain a fabric modified with dopamine hydrochloride;

[0052] Step 3, ultrasonically dispersing the single-walled carbon nanotubes in N,N-dimethylformamide at a ratio of 0.3 g:1 L to obtain solution A;

[0053] Step 4, fixing the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying at 80° C. to obtain a fabric with photoelectric thermal conversion function;

[0054] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and the PDMS curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0055] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 80° C. to obtain a CNT / PDMS-treated fabric;

[0056] Step 7, taking nano ZnO@ZIF-8@SiO2, methacrylate and deionized water in a mass ratio of 3:8:3, and ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution B;

[0057] Step 8: spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 80° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0058] from Figure 1 It can be seen that the water contact angle of the fabric prepared in Example 3 is 152.8°, and thus the fabric has good hydrophobicity. Good hydrophobicity makes its surface less likely to be contaminated by pollutants, thereby increasing the durability of the fabric.

[0059] from Figure 2 It can be seen that the reflectivity of the back side of the fabric prepared in Example 3 to the ultraviolet-visible-near infrared solar light band between 0.5 μm and 1.3 μm is 95% to 98%, and it has good radiation cooling performance.

[0060] from Figure 3 It can be seen that the reflectivity of the front side of the fabric prepared in Example 3 to the ultraviolet-visible-near infrared solar light band between 0.5 μm and 1.3 μm is 5% to 8%, which has a good absorptivity and thus has a good light-to-heat conversion function.

[0061] from Figure 4 It can be seen that the front side of the fabric (ZZS) prepared in Example 3 can be heated up by 18°C ​​under the sun, and the temperature of the leavened surface can be reduced by 6.1°C, while the temperature of the ordinary fabric (unfinished fabric) can only be reduced by about 1.1°C. In addition, when the applied voltage of the fabric prepared in Example 3 is 8V, the current is 0.022A, and the heating temperature can reach 40°C at room temperature, which has good electrothermal conversion performance.

[0062] Example 4

[0063] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 120°C to obtain a clean fabric base;

[0064] Step 2, placing a clean fabric substrate into a dopamine hydrochloride solution with a concentration of 9 mmol / mL and a pH value of 8.5, immersing for 24 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 120° C. to obtain a fabric modified with dopamine hydrochloride;

[0065] Step 3, ultrasonically dispersing graphene in isopropanol at a ratio of 0.4 g:1 L to obtain solution A;

[0066] Step 4, fixing the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying at 120° C. to obtain a fabric with photoelectric thermal conversion function;

[0067] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and the PDMS curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0068] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 120° C. to obtain a CNT / PDMS-treated fabric;

[0069] Step 7, taking nano ZnO@ZIF-8@SiO2, cyanoacrylate and deionized water in a mass ratio of 1:8:2, and ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution B;

[0070] Step 8: spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 120° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0071] Example 5

[0072] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 130°C to obtain a clean fabric base;

[0073] Step 2, placing a clean fabric substrate into a dopamine hydrochloride solution with a concentration of 9 mmol / mL and a pH value of 8.5, immersing for 18 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 130° C. to obtain a fabric modified with dopamine hydrochloride;

[0074] Step 3, ultrasonically dispersing graphene oxide in anhydrous ethanol at a ratio of 0.5 g:1 L to obtain solution A;

[0075] Step 4, fixing the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying at 130° C. to obtain a fabric with photoelectric thermal conversion function;

[0076] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and the PDMS curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0077] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 130° C. to obtain a CNT / PDMS-treated fabric;

[0078] Step 7, taking nano ZnO@ZIF-8@SiO2, cyanoacrylate and deionized water in a mass ratio of 1:8:3, and ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution B;

[0079] Step 8: Spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 130° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0080] Example 6

[0081] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 70°C to obtain a clean fabric base;

[0082] Step 2, placing a clean fabric substrate in a dopamine hydrochloride solution with a concentration of 8 mmol / mL and a pH value of 8.5, immersing for 22 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 70° C. to obtain a fabric modified with dopamine hydrochloride;

[0083] Step 3, ultrasonically dispersing carbon black in N,N-dimethylformamide at a ratio of 0.25 g:1 L to obtain solution A;

[0084] Step 4, fixing the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying at 70° C. to obtain a fabric with photoelectric thermal conversion function;

[0085] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0086] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 70° C. to obtain a CNT / PDMS-treated fabric;

[0087] Step 7, taking nano ZnO@ZIF-8@SiO2, cyanoacrylate and deionized water in a mass ratio of 2:8:3, and ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution B;

[0088] Step 8: Spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 70° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0089] Example 7

[0090] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 90°C to obtain a clean fabric base;

[0091] Step 2, placing a clean fabric substrate in a dopamine hydrochloride solution with a concentration of 8 mmol / mL and a pH value of 8.5, immersing for 14 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 90° C. to obtain a fabric modified with dopamine hydrochloride;

[0092] Step 3, ultrasonically dispersing the single-walled carbon nanotubes in anhydrous ethanol at a ratio of 0.5 g:1 L to obtain solution A;

[0093] Step 4, fixing the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying at 90° C. to obtain a fabric with photoelectric thermal conversion function;

[0094] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and the PDMS curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0095] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 90° C. to obtain a CNT / PDMS-treated fabric;

[0096] Step 7, taking nano ZnO@ZIF-8@SiO2, cyanoacrylate and deionized water in a mass ratio of 2:8:1, and ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution B;

[0097] Step 8: Spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 90° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

[0098] Example 8

[0099] Step 1: Use deionized water and anhydrous ethanol to remove 6×6cm 2 The fabric base is rinsed alternately, and then placed in an oven to dry at 110°C to obtain a clean fabric base;

[0100] Step 2, placing a clean fabric substrate into a dopamine hydrochloride solution with a concentration of 10 mmol / mL and a pH value of 8.5, immersing for 11 hours, taking it out and washing it with deionized water, and then placing it in an oven and drying it at 110° C. to obtain a fabric modified with dopamine hydrochloride;

[0101] Step 3, ultrasonically dispersing the multi-walled carbon nanotubes in isopropanol at a ratio of 0.1 g: 1 L to obtain solution A;

[0102] Step 4, fixing the single-walled carbon nanotubes in solution A on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying at 110° C. to obtain a fabric with photoelectric thermal conversion function;

[0103] Step 5, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and the PDMS curing agent in tetrahydrofuran, and performing ultrasonic dispersion at room temperature until a uniform and transparent PDMS solution is formed;

[0104] Step 6, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and curing at 110° C. to obtain a CNT / PDMS-treated fabric;

[0105] Step 7, taking nano ZnO@ZIF-8@SiO2, methacrylate and deionized water in a mass ratio of 3:8:2, and ultrasonically dispersing the nano ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution B;

[0106] Step 8: spray the mixed solution B on the reverse side of the CNT / PDMS treated fabric, and dry it at 110° C. to obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

Claims

1. A method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions, characterized in that: The steps include: Step 1, first rinse the fabric substrate and dry it, then immerse it in a dopamine hydrochloride solution, take it out, wash it and dry it, to obtain a fabric modified with dopamine hydrochloride; Step 2, dispersing the carbon nanomaterial in an organic solvent according to a ratio (0.1-0.5 g): 1 L, and then fixing the carbon nanomaterial on the front side of the fabric modified with dopamine hydrochloride by suction filtration, and drying to obtain a fabric with photoelectric thermal conversion function; Step 3, weighing PDMS prepolymer, PDMS curing agent and tetrahydrofuran in a mass ratio of 10:1:500, dissolving the PDMS prepolymer and PDMS curing agent in tetrahydrofuran, and fully dispersing them at room temperature until a uniform and transparent PDMS solution is formed; Step 4, immersing the fabric with photoelectric thermal conversion function in a PDMS solution, and obtaining a CNT / PDMS-treated fabric after curing; Step 5, taking nano ZnO@ZIF-8@SiO2, a binder and deionized water in a mass ratio of (1-3):8:(1-3), and then dispersing the ZnO@ZIF-8@SiO2 and the binder in the deionized water to obtain a mixed solution; Step 6: spray the mixed solution on the reverse side of the CNT / PDMS treated fabric, and after drying, obtain a fabric with radiation cooling and photoelectric thermal conversion functions.

2. The method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions according to claim 1, characterized in that: The rinsing in step 1 uses deionized water and anhydrous ethanol to rinse the fabric substrate alternately.

3. The method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions according to claim 1, characterized in that: The fabric base in step 1 is pure cotton fabric.

4. The method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions according to claim 1, characterized in that: The concentration of the dopamine hydrochloride solution in step 1 is (8-10) mmol / mL, the pH value is 8.5, and the immersion time is 12-24 hours.

5. The method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions according to claim 1, characterized in that: The carbon nanomaterial in step 2 is one of single-walled carbon nanotubes, multi-walled carbon nanotubes, MXene, graphene, graphene oxide or carbon black.

6. The method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions according to claim 1, characterized in that: The organic solvent in step 2 is N,N-dimethylformamide, isopropanol or anhydrous ethanol.

7. The method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions according to claim 1, characterized in that: The adhesive in step 5 is methacrylate or cyanoacrylate.

8. The method for preparing a fabric having radiation cooling and photoelectric thermal conversion functions according to claim 1, characterized in that: The drying temperatures of step 1, step 2 and step 6 and the curing temperature of step 4 are all 60-130°C.

9. A fabric having radiation cooling and photoelectric thermal conversion functions prepared by the method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Production method of ZnO nanometer material fabric and ZnO nanometer material fabric

    CN106192420A

  • Preparation method of temperature-responsive self-repairing super-hydrophobic fabric

    CN109576997A

  • Preparation method of dual-mode super-hydrophobic radiation cooling film

    CN114316354A

  • Preparation method and application of durable sensing antibacterial composite fabric and strain sensor

    CN115058898A

  • Nanometer ZnO (at) ZIF-8 (at) SiO2 modified fabric with passive radiation cooling property and after-finishing method of nanometer ZnO (at) ZIF-8 (at) SiO2 modified fabric

    CN115198510A