A gas phase ultra-stable reactor, a device and a method for improving the silicon-aluminum ratio of a catalytic cracking catalyst

By designing a gas phase ultra-stable reactor in the catalytic cracking catalyst and using zone diameter reduction and atomizer technology, the problem of uneven contact between the catalyst and silicon tetrachloride and underdeveloped mesopores was solved, and the reaction efficiency and catalyst crystallization were improved. degree, achieving efficient isomorphous substitution reactions.

CN115805046BActive Publication Date: 2024-10-01PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111083774.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-15
Publication Date
2024-10-01
Estimated Expiration
2041-09-15

AI Technical Summary

Technical Problem

In catalytic cracking catalysts, the contact between the catalyst and silicon tetrachloride in the isomorphous substitution reaction is uneven and the mesopores are underdeveloped, resulting in low reaction efficiency.

Method used

A gas-phase ultra-stable reactor was designed. Through the zone diameter changing reaction and the feed atomizer, the flow rate of the catalyst was changed to improve the contact efficiency between silicon tetrachloride and the catalyst, and the gas-solid phase reaction principle of the down-moving bed mode was adopted. Ensure reaction uniformity and efficiency.

Benefits of technology

The uniformity of the reaction between the catalyst and silicon tetrachloride is achieved, the reaction efficiency is improved, the problems of catalyst backmixing and uneven particle distribution are overcome, and the quality of the isomorphous substitution reaction and the crystallinity retention rate of the catalyst are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115805046B_ABST
    Figure CN115805046B_ABST
Patent Text Reader

Abstract

The present invention relates to a gas phase ultra-stable reactor, which is divided into a buffer zone and a reaction zone from top to bottom, a catalyst inlet is provided at the top of the buffer zone, an atomizer connected to the catalyst inlet is provided at the upper part of the buffer zone, a nitrogen inlet carrying silicon tetrachloride is provided at the bottom of the reaction zone, a discharge port is provided at the upper part of the reaction zone, the inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 4:1, the height of the buffer zone and the reaction zone are independently 0.2 to 1 meter, and the weight ratio of the silicon tetrachloride to the catalyst when reacting in the reaction zone is 0.01 to 0.5:1. The present invention also relates to a device and method for improving the silicon-aluminum ratio of a catalytic cracking catalyst. The gas phase ultra-stable reactor provided by the present invention has the advantages of more complete material contact and high reaction efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalytic cracking catalysts, and in particular relates to a gas phase ultra-stable reactor, and a device and method for improving the silicon-aluminum ratio of a catalytic cracking catalyst. Background Art

[0002] In catalytic cracking catalysts, the stability of molecular sieves, i.e., active components, is crucial to the performance of the catalyst in a catalytic cracking unit. In order to achieve a high silicon-to-aluminum ratio of molecular sieves in the catalyst and improve catalyst stability, the ammonium fluorosilicate method, hydrothermal method, and vapor phase chemical method (also known as vapor phase ultra-stable method) are usually used to extract aluminum and replenish silicon.

[0003] The ammonium fluorosilicate method of aluminum extraction and silicon replenishment (also known as chemical aluminum extraction and silicon replenishment) mainly uses ammonium fluorosilicate to dealuminate and replenish silicon. The obtained molecular sieve has high crystallinity, high Si / Al ratio and thermal stability, but the insoluble AlF3 and residual fluorosilicate formed during the dealuminate process affect the hydrothermal stability and also pollute the environment.

[0004] The hydrothermal method is still a commonly used method in industry. However, the untimely silicon replenishment after dealumination during the hydrothermal process can easily cause lattice collapse and block the pores with non-framework aluminum fragments, which not only affects the accessibility of the active center, but also affects the further improvement of its thermal stability.

[0005] The method of extracting aluminum and replenishing silicon by gas phase chemical method is another important method for preparing high silicon zeolite, which was first reported by Beyer and Mankui in 1980. The gas phase chemical method generally uses SiCl4 under nitrogen protection to react with anhydrous NaY zeolite at a certain temperature. The entire reaction process makes full use of the external Si source provided by SiCl4, and completes the dealumination and silicon replenishment reaction at one time through isomorphous substitution. Therefore, it can effectively avoid the generation of hydroxyl vacancies, lattice collapse, and structural defects when NaY zeolite is dealumination and silicon replenishment reaction under the condition of water vapor, so as to prepare high crystallinity retention rate, high thermal and hydrothermal stability, and high silicon-aluminum ratio high silicon Y-type zeolite. It has the characteristics of uniform dealumination, timely silicon replenishment, high product crystal retention, good thermal stability, and unobstructed pores, becoming an important preparation method for preparing high silicon-aluminum ratio molecular sieves. The core of implementing the good effect of gas phase chemical extraction of aluminum and silicon replenishment lies in the design of gas-solid phase reaction device.

[0006] In terms of gas phase ultra-stable equipment design, CN101884897A, CN101081369A and CN1683245A disclose a gas phase aluminum extraction and silicon supplementation method for molecular sieves, which is carried out in a reaction device, which includes a reactor, a feed port and a gas outlet, a stirrer is included inside the reactor, and a gas-solid separator is installed at the gas outlet. This method makes the contact reaction between silicon tetrachloride gas and molecular sieve solid particles more uniform, effectively avoids the phenomenon of molecular sieve solid particles agglomerating into dense blocks, reduces labor intensity and environmental pollution to a certain extent, and reduces production costs.

[0007] CN102452661A, CN102452660A, CN102452659A, CN102452658A, CN102452657A, CN102451736A, CN102451732A, CN102451730A, CN102451730A, CN102451658A, CN102451657A and CN102451655A respectively designed equipment for gas phase reaction of molecular sieve, the equipment includes a tubular reactor, a gas-solid separator and an absorption tower, the tubular reactor includes a heater, a first feed port, a discharge port and a tube body. The heater can heat the tube body. The key points of this type of invention are, first, adjusting the length of the reaction tube to control the reaction depth, and second, the reaction tube is equipped with a heating device to achieve effective heating of the reaction.

[0008] CN206285918U, CN206285917U and CN206285916U respectively disclose a complete set of equipment and method for preparing catalytic cracking catalyst. The equipment includes a molecular sieve exchange device, a dual-function roasting furnace, a gas-phase ultra-stable reactor, a gas-solid separation device, a gelling device, and a drying roasting unit. The dual-function roasting furnace includes a furnace body and a cylinder arranged in the furnace body, and the cylinder includes a feed end, an intermediate cylinder and a discharge end in sequence. Along the direction of the material, the roasting furnace also includes a water vapor distributor for providing water vapor in the cylinder and a dry gas distributor for providing dry gas as a drying roasting medium in the cylinder. The gas-phase ultra-stable reaction device of the above invention is an inclined tube reactor.

[0009] CN109092217A and CN109092217B respectively disclose a gas-phase ultra-stable reactor for chemical production, which is aimed at the problems of poor sealing in the first, second and third stages of the reactor in the invention 201710359787.4, the need for repositioning during the overhaul and maintenance process, and the low efficiency of the overhaul and maintenance. The sealing performance of the reactor is enhanced, the impact on the reactor after disassembly is reduced, and the quality of disassembly and assembly is improved. The high silicon-aluminum ratio Beta molecular sieve prepared by CN111017948A adopts a horizontal reactor.

[0010] CN102049315A introduces the method of controlling the flow rate of carrier gas and the length of tubular reactor to control the time of molecular sieve and SiCl4 contact, so that the contact reaction of molecular sieve and SiCl4 can be fully carried out in tubular reactor. But in this application, gas is adopted to carry molecular sieve powder material and SiCl4 gas contact reaction mode to carry out gas phase ultra-stable reaction, and the weight ratio of carrier gas to SiCl4 reaches 10-250, causing SiCl4 to be excessive, which not only aggravates the harm of environmental pollution but also is more unfavorable for the effective absorption of tail gas. CN201210418208.6CN201210417927.6, CN201210417732.1, CN201210418185.9 respectively introduce the process of continuous preparation of high silicon molecular sieve, comprising molecular sieve exchange device, roasting furnace, gas phase ultra-stable reactor and gas-solid separation device, wherein the gas phase ultra-stable reactor is a tilted tubular furnace with a certain angle to the horizontal, and the molecular sieve flows slowly. In CN201010515244.5, CN200910236629.5, CN200910236629.5, CN201010515420.5, and CN201010515213.X, the molecular sieve undergoes gas phase reaction in a tubular reactor, and silicon tetrachloride gas and the molecular sieve flow in the same direction for reaction. CN201811279376.5, CN201821779273.0, and CN201811279418.5 respectively disclose a process for gas phase ultrastable modification of molecular sieves, wherein the reactor is horizontally divided into several different functional areas to complete the reaction.

[0011] Chinese application CN201621178825.3 discloses a device for preparing catalytic cracking catalyst. The device includes a Na-type molecular sieve exchange device, a dual-function roasting furnace, a gas-phase ultra-stable reactor, a gas-solid separation device, a washing and filtering unit, and a gelling device; a drying and roasting unit is used to dry and roast the slurry; the dual-function roasting furnace includes a furnace body and a cylinder arranged in the furnace body, and the cylinder sequentially includes a feed end, an intermediate cylinder and a discharge end. Along the direction of the material, the roasting furnace also includes a water vapor distributor sequentially arranged in the cylinder for providing water vapor in the cylinder and a dry gas distributor for providing a dry roasting medium in the cylinder. However, the gas-phase ultra-stable reactor in the invention is a tubular reactor or a conveyor bed reactor (moving bed reactor), and the material silicon tetrachloride can share an inlet with the molecular sieve inlet or enter the reactor in the same direction for reaction, which has the problem of uneven material mixing and low reaction efficiency.

[0012] Chinese application CN201611116722.9 discloses a device for preparing low-sodium and high-silicon-aluminum ratio Y-type molecular sieve, the device comprising a reactor, a first feed channel and a discharge channel opening at the upper part of the reactor, a second feed channel opening at the lower part of the reactor, a mixing device located at the lower part of the reactor, a reaction component located inside the reactor, a heating device for supplying heat to the reactor, a gas-solid separation device connected to one end of the discharge channel, and a heat storage device evenly distributed in the reactor; the reactor comprises at least one group of reaction components evenly distributed in the middle thereof, the top end of the reaction component is connected to the other end of the discharge channel, the bottom end is connected to the upper part of the mixing device, the lower part of the mixing device is connected to the first feed channel, and the middle part is connected to the second feed channel; the reaction component comprises at least one fluidized bed. Although the gas-phase ultrastable reactor in this invention adopts a fluidized bed reactor, the molecular sieve raw powder is transported to the lower part of the reactor using a dry carrier gas, mixed with halogen silane and then enters the reaction component in the reactor for reaction, and finally discharged from the upper part of the reactor. The material and halogen silane are fed in the same direction, which may also bring about problems of uneven material mixing and low reaction efficiency. Summary of the invention

[0013] Based on the above, the main purpose of the present invention is to provide a gas-phase ultra-stable reactor, so as to solve the problems of uneven contact between catalyst and silicon tetrachloride, underdeveloped mesopores and low reaction efficiency in isomorphous substitution reaction.

[0014] Another object of the present invention is to provide an apparatus and method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst.

[0015] In order to achieve the above-mentioned purpose, the present invention provides a gas phase ultra-stable reactor, which is divided into a buffer zone and a reaction zone from top to bottom, a catalyst inlet is provided at the top of the buffer zone, an atomizer connected to the catalyst inlet is provided at the upper part of the buffer zone, a nitrogen inlet carrying silicon tetrachloride is provided at the bottom of the reaction zone, a discharge port is provided at the upper part of the reaction zone, the inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 4:1, the height of the buffer zone and the reaction zone are independently 0.2 to 1 meter, and the weight ratio of the silicon tetrachloride to the catalyst when reacting in the reaction zone is 0.01 to 0.5:1.

[0016] Specifically, the present invention can change the flow rate of the catalyst and improve the efficiency of contact with silicon tetrachloride through the design of the zone variable diameter reaction and the feed atomizer in the reactor design, thereby ensuring the uniformity of the reaction between the material and silicon tetrachloride and improving the reaction efficiency. At the same time, according to the characteristics of the catalytic cracking catalyst microsphere particles, the gas-solid phase reaction principle of the descending bed mode is adopted to design a device suitable for the isomorphous substitution reaction of the microsphere catalyst. The material descends along the gravity field, and SiCl4 contacts the material from bottom to top under the action of the carrier gas. This contact mode can not only effectively overcome the problems of catalyst back mixing and uneven distribution of catalyst particles along the radial direction caused by the operation of the ascending riser against gravity, but also realize the ultra-short contact operation of the material and the reactant due to the increase of the gas-solid two-phase flow rate, and the reaction is uniform, so the excellence of the reaction effect is very prominent, and it is very suitable for gas and solid phase rapid processing reaction process. The in-situ crystallization catalyst obtained by the above design has the characteristics of high crystallinity retention rate, high activity, and more significant reduction of sodium oxide.

[0017] The gas phase ultrastable reactor described in the present invention, wherein preferably, the inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 3:1; further preferably, a heating jacket or a heating belt is provided on the outer wall of the gas phase ultrastable reactor; further preferably, the cavity diameter of the buffer zone is 0.05 to 0.5 meters, and the height is 0.2 to 1 meter.

[0018] The gas phase ultrastable reactor described in the present invention is preferably that the atomizer is made of stainless steel, contains a plurality of symmetrically distributed air holes, the diameter of the air holes is 80 to 200 um, and the gas pressure inside the atomizer is 0.1 to 6 MPa.

[0019] In order to achieve the above object, the present invention also provides a device for improving the silicon-aluminum ratio of a catalytic cracking catalyst, comprising:

[0020] A pretreatment furnace, used for calcining or hydrothermal treatment of the catalyst to obtain a pretreated catalyst;

[0021] The above-mentioned gas phase ultrastable reactor is used to carry out isomorphous substitution reaction on the pretreated catalyst to obtain the reacted catalyst;

[0022] The absorption tower is used to blow the reacted catalyst from the feed port into the absorption tower, and then the tail gas neutralization reaction occurs to obtain the catalyst intermediate;

[0023] Exchange filter, used for exchange and filtration of catalyst intermediates;

[0024] Flash drying equipment, used for flash evaporation and drying of catalyst intermediates.

[0025] The device for improving the silicon-aluminum ratio of the catalytic cracking catalyst described in the present invention preferably also includes a recovery system for recovering the nitrogen carrying silicon tetrachloride in the gas phase ultrastable reactor.

[0026] The device for improving the silicon-aluminum ratio of catalytic cracking catalyst described in the present invention is preferably that the pretreatment furnace comprises a feeding section, a roasting section and a discharging section, the total length of the pretreatment furnace is 0.5 to 5 meters, the inner diameter is 0.01 to 1 meter, and the roasting temperature is 100 to 1000°C.

[0027] The device for improving the silicon-to-aluminum ratio of catalytic cracking catalyst described in the present invention, wherein preferably, the pretreatment furnace includes a heating system and a ventilation system, the heating system is arranged on the outer layer of the pretreatment furnace in the form of a furnace tile jacket, and the ventilation system is arranged on the inner wall of the pretreatment furnace, and the ventilation system can input dry gas, nitrogen or water vapor into the interior of the pretreatment furnace, so as to realize flexible switching between conventional roasting and water vapor roasting.

[0028] The device for improving the silicon-to-aluminum ratio of catalytic cracking catalyst described in the present invention is preferably such that the angle α between the pretreatment furnace feed section and the pretreatment furnace body is greater than 10° and less than 90°, and the angle β between the pretreatment furnace body and the horizontal position is greater than 10° and less than 90°.

[0029] The device for improving the silicon-aluminum ratio of catalytic cracking catalyst described in the present invention is preferably provided with an axis rotating device on the top of the pretreatment furnace to control the rotation of the furnace body of the pretreatment furnace, and the rotation frequency is 10 to 80 Hz / min.

[0030] In order to achieve the above object, the present invention also provides a method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst, based on the above-mentioned device for increasing the silicon-aluminum ratio of a catalytic cracking catalyst, comprising the following steps:

[0031] S1. The catalyst is calcined or hydrothermally treated in a pretreatment furnace to obtain a pretreated catalyst;

[0032] S2. The pretreated catalyst enters a gas-phase ultrastable reactor and contacts with nitrogen carrying silicon tetrachloride to undergo an isomorphous substitution reaction, wherein the weight ratio of silicon tetrachloride to the catalyst is 0.01 to 0.5:1. Through this isomorphous substitution reaction, the catalyst can achieve the goal of rapidly reducing the sodium oxide content and retaining the crystallinity to the maximum extent.

[0033] S3. The catalyst after the reaction is purged, collected, and washed with water in an absorption tower, and then ammonium-free exchange, washing, and drying are performed to obtain a finished product.

[0034] Specifically, the device and method of the present invention first adopt an in-situ crystallization process to prepare a catalyst with a molecular sieve content of 5 to 60wt%. Then, in order to address the defect of underdeveloped pore structure of the isomorphous substitution catalyst, a pretreatment furnace that can be used for conventional roasting or steam roasting is added in front of the isomorphous substitution reaction device. This pretreatment furnace treatment method can flexibly adjust the catalyst pore structure as needed to achieve multiple functions.

[0035] Specifically, the device and method of the present invention connects an absorption tower at the rear end of the reactor to purge excess silicon tetrachloride and acidic gas adsorbed on the catalyst surface, reducing the impact of excess silicon tetrachloride on the catalyst and effectively ensuring the quality of isomorphous substitution. The in-situ crystallization catalyst obtained by the above design has the characteristics of high crystallinity retention rate, high activity, and more significant reduction of sodium oxide.

[0036] The method for improving the silicon-aluminum ratio of a catalytic cracking catalyst described in the present invention preferably further includes the following steps: S4, the gas after the reaction enters a recovery system, the alkaline solution in the recovery system is at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate, and the concentration of the alkaline solution is 1 to 20 wt%.

[0037] The method for improving the silicon-aluminum ratio of catalytic cracking catalysts of the present invention is preferably such that after the catalyst passes through a pretreatment furnace, the pretreated catalyst has a ignition loss of less than 3wt% and a Y-type molecular sieve content of 5-60wt%.

[0038] The method for improving the silicon-aluminum ratio of a catalytic cracking catalyst of the present invention is preferably such that, in the gas phase ultrastable reactor, the temperature is 200-900° C., the contact time between the catalyst and silicon tetrachloride gas is 0.1-60 min, the weight ratio of the catalyst to silicon tetrachloride gas is 0.01-0.5:1, and the volume ratio of silicon tetrachloride to nitrogen in the nitrogen carrying silicon tetrachloride is 0.1-100:1.

[0039] In the method for improving the silicon-aluminum ratio of catalytic cracking catalyst described in the present invention, it is preferred that the inner diameter of the absorption tower is 1 to 50 cm, and the time for passing gas to purge the material is 10 to 120 minutes.

[0040] The method for improving the silicon-aluminum ratio of a catalytic cracking catalyst of the present invention is preferably that the catalyst is prepared by an in-situ crystallization process; specifically, the catalyst is prepared by the following method: kaolin, a dispersant and / or a reinforcing agent, and deionized water are mixed and slurried to obtain a slurry, wherein the solid content of the slurry is 30-50wt%; the slurry is spray-dried to prepare spray microspheres with a particle size of 20-110μm, and calcined at 600-1000°C for 1-3h to obtain calcined microspheres; the calcined microspheres, sodium silicate, a directing agent, a sodium hydroxide solution, and deionized water are mixed, crystallized at 85-95°C for 16-36h, the mother liquor is filtered to remove, the filter cake is washed with deionized water until the pH is below 10.5, and the catalyst is obtained after drying, wherein the catalyst contains 5-60wt% NaY molecular sieve, and the amount of the dispersant and / or reinforcing agent added is 1-20wt% of the total mass of the kaolin. The catalyst prepared by the above method has good pore structure and anti-wear performance. There is no limitation on the order of adding the dispersant and the reinforcing agent, and they can be added simultaneously or in batches.

[0041] The method for improving the silicon-aluminum ratio of catalytic cracking catalyst described in the present invention is preferably that the kaolin includes soft kaolin and hard kaolin, the median diameter of the kaolin is 1.5-3.0 μm, the crystalline kaolinite content is higher than 80wt%, the iron oxide is lower than 1.7wt%, and the sum of sodium oxide and potassium oxide is lower than 0.5wt%.

[0042] The method for improving the silicon-aluminum ratio of catalytic cracking catalyst described in the present invention is preferably that the dispersant includes one of sodium silicate and sodium pyrophosphate, and the added amount of the dispersant is 1-20% of the mass of kaolin, and more preferably 1-15%; the reinforcing agent includes one of silica sol and aluminum sol, and the added amount is 1-20% of the mass of kaolin, and more preferably 2-8%.

[0043] In the method for improving the silicon-aluminum ratio of the catalytic cracking catalyst of the present invention, it is preferred that the calcination temperature is 600-850°C or 860-1000°C. That is, the microspheres are calcined at a temperature of 600-1000°C, and low-temperature calcined microspheres can be obtained by calcining at 600-850°C for 1-3 hours, or high-temperature calcined microspheres can be obtained by calcining at 860-1000°C for 1-3 hours, or a mixture of low-temperature calcined microspheres and high-temperature calcined microspheres.

[0044] The method for improving the silicon-aluminum ratio of the catalytic cracking catalyst described in the present invention has no special restrictions on the composition of the directing agent. A common directing agent can be used. For example, the directing agent composition is prepared according to Example 1 of CN1232862A. Preferably, the components and molar ratio of the directing agent are (14-16)SiO2:(0.7-1.3)Al2O3:(14-16)Na2O:(300-330)H2O.

[0045] In the method for improving the silicon-aluminum ratio of a catalytic cracking catalyst of the present invention, it is preferred that the catalyst in step S1 is an unmodified sodium-type intermediate product or a hydrogen-type product after modified ion exchange.

[0046] The method for improving the silicon-aluminum ratio of a catalytic cracking catalyst of the present invention is preferably that the washing step is: adding the catalyst to an exchange tank, adding deionized water and stirring evenly, and then starting washing to obtain a slurry; further preferably, the washing conditions are: a mass ratio of the catalyst to H2O of 1:1-25, a slurry pH of 2.5-8.5, a washing temperature of 30-95°C, and a washing time of 0.5-2h.

[0047] The method for improving the silicon-aluminum ratio of a catalytic cracking catalyst described in the present invention is preferably that the ammonium-free exchange is an acid exchange, and further preferably, the acid exchange step is: adding the catalyst to an exchange tank, adding an acid solution and deionized water, stirring evenly to obtain a slurry and performing the exchange; further preferably, the acid exchange conditions are: the slurry pH value is 3-6, the temperature is 80-95°C, the acid of the acid solution is selected from one or more of sulfuric acid, oxalic acid, hydrochloric acid, phosphoric acid, and nitric acid, and hydrochloric acid and / or nitric acid are further preferred, and the exchange time is 20-60 minutes.

[0048] The beneficial effects of the present invention are as follows:

[0049] (1) The reactor provided by the present invention has more complete material contact and high reaction efficiency: according to the characteristics of the catalytic cracking catalyst microsphere particles, the gas-solid phase reaction principle of the descending bed mode is adopted, the material descends along the gravity field, and SiCl4 contacts the material from bottom to top under the action of the carrier gas. This contact mode can not only effectively overcome the problems of catalyst back mixing and uneven radial distribution of catalyst particles caused by the operation of the ascending riser against gravity, but also realize ultra-short contact operation between the material and the reactant due to the increase in the gas-solid two-phase flow rate, and the reaction is uniform, so the excellent reaction effect is very outstanding, which is very suitable for the gas and solid phase rapid processing reaction process.

[0050] (2) The reactor provided by the present invention improves the efficiency of isomorphous substitution reaction: in the design of the reactor, the flow rate of the catalyst can be changed and the efficiency of contact with silicon tetrachloride can be improved through the design of zoned variable diameter reaction and feed atomizer, thereby ensuring the uniformity of the reaction between the material and silicon tetrachloride and improving the reaction efficiency.

[0051] (3) The device provided by the present invention can make up for the defect of underdeveloped mesoporous volume of the catalyst: a pretreatment furnace that can be used for conventional calcination or steam calcination is added before the isomorphous substitution reaction device. This pretreatment furnace treatment method can flexibly adjust the catalyst pore structure as needed, thereby increasing the mesoporous volume of the catalyst.

[0052] (4) The device provided by the present invention has high quality of isomorphous substitution reaction: an absorption tower is connected to the rear end of the reactor to purge excess silicon tetrachloride and acidic gas adsorbed on the catalyst surface, thereby reducing the impact of excess silicon tetrachloride on the catalyst and effectively ensuring the quality of isomorphous substitution. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 Schematic diagram of the structure of the gas phase ultrastable reactor.

[0054] Figure 2 It is a schematic structural diagram of the device for improving the silicon-aluminum ratio of catalytic cracking catalyst according to the present invention.

[0055] Figure 3 It is the angle between the pretreatment section and the pretreatment furnace.

[0056] Figure 4 This is a schematic diagram of the structure of the pretreatment furnace.

[0057] Figure 5 This is a schematic diagram of the structure of the absorption tower.

[0058] in:

[0059] 1. Pretreatment furnace, 2. Gas phase ultra-stable reactor, 3. Absorption tower, 4. Exchange, filter and flash drying equipment;

[0060] 11. Feeding section, 12. Roasting section, 13. Discharging section, 14. Shaft rotating device, 15. Heating system, 16. Ventilation system,

[0061] 21. Buffer zone, 22. Reaction zone, 23. Catalyst inlet, 24. Atomizer, 25. Nitrogen inlet carrying silicon tetrachloride, 26. Discharge port, 27. Heating jacket,

[0062] 31. Air inlet, 32. Exhaust gas outlet, 33. Catalyst inlet, 34. Wind agitator. DETAILED DESCRIPTION

[0063] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.

[0064] See also Figure 1As shown, the gas phase ultra-stable reactor 2 provided by the present invention is divided into a buffer zone 21 and a reaction zone 22 from top to bottom, a catalyst inlet 23 is provided at the top of the buffer zone 21, an atomizer 24 connected to the catalyst inlet 23 is provided at the upper part of the buffer zone 21, a nitrogen inlet 25 carrying silicon tetrachloride is provided at the bottom of the reaction zone 22, a discharge port 26 is provided at the upper part of the reaction zone 22, an inner diameter ratio of the buffer zone 21 to the reaction zone 22 is 1:1-4:1, the height of the buffer zone 21 and the reaction zone 22 are independently 0.2-2 meters, and the weight ratio of silicon tetrachloride to the catalyst when reacting in the reaction zone 22 is 0.01-0.5:1.

[0065] Also, see Figure 1 As shown, a heating jacket 27 is provided on the outer wall of the gas phase ultrastable reactor 2. Of course, in other embodiments, the heating jacket 27 can be replaced by other heating structures, such as a heating belt.

[0066] In some embodiments, the cavity diameter of the reaction zone 22 is preferably 0.05 to 0.5 meters, and the height is preferably 0.2 to 1 meter.

[0067] In some embodiments, the inner diameter ratio of the buffer zone 21 to the reaction zone 22 is preferably 1:1 to 3:1.

[0068] In some embodiments, the atomizer 24 is made of stainless steel, and contains a plurality of symmetrically distributed air holes, the diameter of the air holes is 80-200 um, and the gas pressure inside the atomizer 24 is 0.1-6 MPa.

[0069] See also Figure 2 As shown, the device for improving the silicon-aluminum ratio of catalytic cracking catalyst provided by the present invention comprises:

[0070] Pretreatment furnace 1, used for calcination or hydrothermal treatment of catalyst to obtain pretreated catalyst;

[0071] The above-mentioned gas phase ultrastable reactor 2 is used to carry out isomorphous substitution reaction on the pretreated catalyst to obtain the reacted catalyst;

[0072] Absorption tower 3, used to purge the reacted catalyst from the feed port into the absorption tower, and then the tail gas neutralization reaction occurs to obtain a catalyst intermediate;

[0073] The exchange, filter and flash drying equipment 4 includes an exchange filter for exchanging and filtering the catalyst intermediates; and a flash drying device for flashing and drying the catalyst intermediates.

[0074] Also, see Figure 3 As shown, the pretreatment furnace 1 comprises a feeding section 11, a roasting section 12 and a discharging section 13. The total length of the pretreatment furnace 1 is 0.5 to 5 meters, the inner diameter is 0.01 to 1 meter, and the roasting temperature is 100 to 1000°C.

[0075] Also, see Figure 4 As shown, the pretreatment furnace 1 includes a heating system 15 and a ventilation system 16. The heating system 15 is arranged on the outer layer of the pretreatment furnace 1 in the form of a furnace tile jacket, and the ventilation system 16 is arranged on the inner wall of the pretreatment furnace 1. The ventilation system 16 can input dry gas, nitrogen or water vapor into the interior of the pretreatment furnace 1.

[0076] Also, see Figure 3 As shown, the angle α between the feed section 11 of the pretreatment furnace 1 and the main body of the pretreatment furnace 1 is greater than 10° and less than 90°; Figure 4 As shown, the angle β between the main body of the pretreatment furnace 1 and the horizontal position is greater than 10° and less than 90°. The top of the pretreatment furnace 1 is provided with an axis rotating device 14, and the furnace body can rotate to achieve the turning of the material, and the rotation frequency is 10-80Hz / min.

[0077] Also, see Figure 5 As shown, the absorption tower 3 includes an air inlet 31, an exhaust gas outlet 32, a catalyst inlet 33 and a wind stirrer 34, and the exhaust gas outlet 32 ​​is 2 to 10 cm away from the top of the reactor. The reacted catalyst enters the absorption tower 3 through the catalyst inlet 33, and under the action of the wind stirrer 34, it reacts with the exhaust gas entering through the air inlet 31 to obtain a catalyst intermediate. After the reaction is completed, the catalyst intermediate is discharged from the absorption tower 3 through the discharge port (not shown) at the bottom of the absorption tower, and the reacted exhaust gas is discharged from the absorption tower 3 through the exhaust gas outlet 32 ​​after being pumped and enters the recovery system.

[0078] In some embodiments, the device for improving the silicon-to-aluminum ratio of a catalytic cracking catalyst provided by the present invention further includes a recovery system for recovering nitrogen carrying silicon tetrachloride in the gas-phase ultrastable reactor 2 .

[0079] Combination Figure 2 As shown, the method for improving the silicon-aluminum ratio of the catalytic cracking catalyst provided by the present invention is based on the above-mentioned device for improving the silicon-aluminum ratio of the catalytic cracking catalyst, comprising the following steps:

[0080] S1, the catalyst is calcined or hydrothermally treated in a pretreatment furnace 1 to obtain a pretreated catalyst;

[0081] S2, the pretreated catalyst is transported to the catalyst inlet 23 of the gas phase ultra-stable reactor 2 by a hoist and enters the atomizer 24, and after atomization, enters the reaction zone 22 to contact with nitrogen carrying silicon tetrachloride to undergo isomorphous substitution reaction, and the weight ratio of silicon tetrachloride to catalyst is 0.01-0.5:1;

[0082] S3. The reacted catalyst is purged, collected, and washed with water in the absorption tower 3, and then subjected to ammonium-free exchange, washing, and drying to obtain a finished product.

[0083] In some embodiments, the method provided by the present invention also includes the following steps: S4, the gas after the reaction enters a recovery system, the gas after the reaction contains excess silicon tetrachloride, hydrochloric acid and reacted aluminum chloride, the alkaline solution in the recovery system is at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate, and the concentration of the alkaline solution is 1 to 20wt%.

[0084] In some embodiments, after the catalyst passes through the pretreatment furnace 1, the pretreated catalyst has a burn-off within 3 wt% and a Y-type molecular sieve content of 5 to 60 wt%.

[0085] In some embodiments, the temperature in the gas phase ultrastable reactor 2 is 200-900° C., the contact time between the catalyst and the silicon tetrachloride gas is 0.1-60 min, the weight ratio of the catalyst to the silicon tetrachloride gas is 0.01-0.5:1, and the volume ratio of silicon tetrachloride to nitrogen in the nitrogen carrying silicon tetrachloride is 0.1-100:1.

[0086] In some embodiments, the inner diameter of the absorption tower 3 is 1 to 50 cm, and the time for passing gas to purge the material is 10 to 120 minutes.

[0087] In some embodiments, the catalyst is prepared by the following method: kaolin, dispersant and / or reinforcing agent, and deionized water are mixed and slurried to obtain a slurry, the solid content of the slurry is 30-50wt%; the slurry is spray-dried to prepare spray microspheres with a particle size of 20-110μm, and calcined at 600-1000℃ for 1-3h to obtain calcined microspheres. The calcined microspheres, sodium silicate, directing agent, sodium hydroxide solution, and deionized water are mixed, crystallized at 85-95℃ for 16-36h, the mother liquor is filtered to remove the mother liquor, the filter cake is washed with deionized water to a pH of less than 10.5, and a catalyst containing 5-60wt% NaY molecular sieve is obtained after drying, and the amount of dispersant and / or reinforcing agent added is 1-20wt% of the total mass of kaolin.

[0088] In some embodiments, the kaolin includes soft kaolin and hard kaolin, the kaolin has a median diameter of 1.5-3.0 μm, a crystalline kaolinite content higher than 80 wt%, iron oxide lower than 1.7 wt%, and a sum of sodium oxide and potassium oxide lower than 0.5 wt%.

[0089] In some embodiments, the dispersant includes one of sodium silicate and sodium pyrophosphate, and the amount of the dispersant added is 1-20% of the mass of kaolin, preferably 1-15%; the reinforcing agent includes one of silica sol and aluminum sol, and the amount of the reinforcing agent added is 1-20% of the mass of kaolin, preferably 2-8%.

[0090] In some embodiments, the calcination temperature is 600-850°C or 860-1000°C.

[0091] In some embodiments, the components and molar ratio of the directing agent are (14-16)SiO2:(0.7-1.3)Al2O3:(14-16)Na2O:(300-330)H2O.

[0092] In some embodiments, the catalyst in step S1 is an unmodified sodium-type intermediate product or a hydrogen-type product after modified ion exchange.

[0093] In some embodiments, the washing step is: adding the catalyst to an exchange tank, adding deionized water and stirring evenly, and then starting washing to obtain a slurry; preferably, the washing conditions are: a mass ratio of the catalyst to H2O of 1:1 to 25, a slurry pH of 2.5 to 8.5, a washing temperature of 30 to 95°C, and a washing time of 0.5 to 2h.

[0094] In some embodiments, the ammonium-free exchange is an acid exchange. Preferably, the acid exchange step is: adding the catalyst to an exchange tank, adding an acid solution and deionized water, stirring evenly to obtain a slurry and performing the exchange; more preferably, the acid exchange conditions are: the slurry pH value is 3-6, the temperature is 80-95°C, the acid of the acid solution is selected from one or more of sulfuric acid, oxalic acid, hydrochloric acid, phosphoric acid, and nitric acid, preferably hydrochloric acid and / or nitric acid, and the exchange time is 20-60 min.

[0095] Source of raw materials:

[0096] (1) Kaolin: industrial product, collected from the catalyst plant of Lanzhou Petrochemical Company.

[0097] (2) Sodium silicate: industrial product, sourced from the catalyst plant of Lanzhou Petrochemical Company.

[0098] (3) High Alkalinity Sodium Aluminate: Industrial product, sourced from the Catalyst Factory of Lanzhou Petrochemical Company.

[0099] (4) NaOH solution: industrial product, obtained from the catalyst plant of Lanzhou Petrochemical Company.

[0100] (5) Hydrochloric acid: chemically pure.

[0101] Specific analysis method:

[0102] (1) Test of Crystallinity of NaY Molecular Sieve The crystallinity of the sample was measured by X-ray diffraction method on a D / max-3C X-ray powder diffractometer manufactured by Rigaku Corporation of Japan, according to the method standard Q / SYLS 0596-2002.

[0103] (2) Testing the silicon-aluminum ratio of NaY molecular sieves The X-ray powder diffraction method is used, and the method standard is Q / SYLS 0573-2002.

[0104] (3) Microreaction activity (MA) evaluation: ASTM-D3907 method was used. The catalyst was pre-treated at 800°C and 100% steam for 17 h. Dagang light diesel was used as the reaction raw oil. The reaction temperature was 460°C, the oil injection time was 70 s, the catalyst loading was 2.5-5 g, and the gasoline yield after the reaction was analyzed by GC7890. Specific embodiment:

[0106] Example 1

[0107] 3000g of kaolin (burning base), 5wt% of sodium silicate (100% of kaolin), 20wt% of silica sol (100% of kaolin), and chemical water were prepared into a mixed slurry with a solid content of 46wt%, and spray-dried to obtain 2300g of spray soil balls with a particle size of 20-110μm. One part of the spray soil balls was roasted at 925℃ for 2.7h, and the other part was roasted at 650℃ for 2.5h. Then, 200g and 300g of the two kinds of soil balls were mixed, and sodium silicate, a directing agent, a sodium hydroxide solution, and chemical water were added. The mixture was hydrothermally crystallized at 95℃ for 30h, and the mother liquor was filtered out, and the product was washed and dried. Dry gas is introduced into the pretreatment furnace. After calcination at 600℃ for 3h, 200g of catalyst containing 60wt% Y-type molecular sieve and 1.2wt% ignition loss is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 200μm and a pressure of 6MPa. After spraying by the atomizer, the catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 100:1, the reaction temperature is 900℃, and the contact time with the gas is 0.1min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to in-situ crystallization catalyst is 0.5:1. The inner diameter of the buffer zone and the reaction zone are both 0.05 meters, and the heights are 0.2 and 0.3 meters respectively. After the reacted material enters the absorption tower for 30min of purge, the reacted gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 10wt% sodium hydroxide solution, and the reacted gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water. The catalyst washed with water: H2O = 1:25, pH value is 8.5, washing temperature is 30°C, and washing time is 0.5h. Then it is exchanged with sulfuric acid, the exchange pH is 3.2, the temperature is 80°C, and the exchange is 1h. The product after the exchange is washed and dried to become cat-1.

[0108] Example 2

[0109] 600g of kaolin (burnt base), 7wt% of sodium pyrophosphate (based on kaolin as 100%), 1wt% of aluminum sol (based on kaolin as 100%), and chemical water are prepared into a mixed slurry with a solid content of 32wt%, and spray-dried to obtain 300g of spray soil balls with a particle size of 20-110μm. The spray soil balls are roasted at 990℃ for 1.5h, sodium silicate, directing agent, sodium hydroxide solution, and chemical water are added, and hydrothermal crystallization is carried out at 85℃ for 16h, the mother liquor is filtered out, and the product is washed and dried. 50wt% water vapor is introduced into the pretreatment furnace. After calcination at 500℃ for 3h, 800g of catalyst containing 5wt% Y-type molecular sieve and ignition loss of 2.2wt% is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 50μm and a pressure of 0.1MPa. After spraying by the atomizer, the catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 0.1:1. The gas-solid phase reaction temperature is 200℃, and the contact time with the gas is 3min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.01:1. The inner diameters of the buffer zone and the reaction zone are 0.5m and 0.125m respectively, and the height is 1m. The reacted material is purged in the absorption tower for 15min. The gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 20wt% sodium carbonate solution, and the reacted gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water. The catalyst washed with water: H2O = 1:20, pH value is 6.5, washing temperature is 50°C, and washing time is 1h. Then it is exchanged with hydrochloric acid, the exchange pH is 4.2, the temperature is 95°C, and the exchange time is 45min. The product after the exchange is washed and dried to become cat-2.

[0110] Example 3

[0111] 1300g of kaolin (burning base), 15wt% of sodium silicate (100% of kaolin), 5wt% of aluminum sol (100% of kaolin), and chemical water were prepared into a mixed slurry with a solid content of 40wt%, and spray-dried to obtain 600g of spray soil balls with a particle size of 20-110μm. The spray soil balls were roasted at 990℃ for 1.5h, sodium silicate, directing agent, sodium hydroxide solution, and chemical water were added, and hydrothermal crystallization was carried out at 85℃ for 16h, the mother liquor was filtered out, and the product was washed and dried. After being calcined at 700℃ for 2h in a pretreatment furnace, 600g of a catalyst containing 40wt% Y-type molecular sieve and ignition loss of 2.8wt% is slowly added to the top of the downward bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 80μm and a pressure of 4MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 10:1. The gas-solid phase reaction temperature is 400℃, and the contact time with the gas is 60min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.3:1. The inner diameters of the buffer zone and the reaction zone are 0.4m and 0.2m respectively, and the heights are 0.5m and 0.2m respectively. The reacted material is purged for 40min, and the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 12wt% sodium hydroxide solution, and the reacted gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water. The catalyst washed with water: H2O = 1:1, pH value is 2.5, washing temperature is 70°C, and washing time is 2.5h. Then it is exchanged with oxalic acid, the exchange pH is 5.1, the temperature is 80°C, and the exchange time is 30min. The product after the exchange is washed and dried to become cat-3.

[0112] Example 4

[0113] 1200g of kaolin (burning base), 19wt% of sodium pyrophosphate (with kaolin as 100%), 16wt% of silica sol and chemical water were prepared into a mixed slurry with a solid content of 47wt%, and spray dried to obtain 1100g of spray soil balls with a particle size of 20-110μm. One part of the spray soil balls was roasted at 1000℃ for 1.5h, and the other part was roasted at 800℃ for 2h, then 800g and 200g of the above soil balls were added with sodium silicate, directing agent, sodium hydroxide solution and chemical water, and hydrothermally crystallized at 89℃ for 30h, the mother liquor was filtered out, and the product was washed and dried. The product is treated with nitric acid, nitric acid / product = 0.07, exchanged at pH = 3.0-4.5, 93 ° C for 1.5 hours, filtered to remove the filtrate, the filter cake is roasted at 700 ° C for 2 hours in the pretreatment furnace, and 500 grams of the catalyst containing 30wt% Y-type molecular sieve and 1.8wt% of ignition reduction is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 150μm and a pressure of 3MPa. After spraying by the atomizer, the catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 0.5:1, the gas-solid phase reaction temperature is 500 ° C, and the contact time with the gas is 30min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.22:1. The inner diameters of the buffer zone and the reaction zone are 0.3 meters and 0.15 meters respectively, and the heights are 0.3 meters and 0.7 meters respectively. The reacted material is purged in the absorption tower for 60 minutes, and the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 15wt% sodium hydroxide solution, which neutralizes and collects the reacted gas. The catalyst is collected by the collector at the bottom of the absorption tower and then washed with water. The washed catalyst: H2O=1:10, pH value is 3.5, washing temperature is 80°C, and washing time is 1.5h. The washed product is washed and dried to become cat-4.

[0114] Example 5

[0115] 1500g of kaolin (burning base), 13wt% of sodium silicate (100% of kaolin), 13wt% of silica sol (100% of kaolin), and chemical water were prepared into a mixed slurry with a solid content of 43wt%, and spray-dried to obtain 1400g of spray soil balls with a particle size of 20-110μm. One part of the spray soil balls was roasted at 970℃ for 2.3h, and the other part was roasted at 850℃ for 1.9h. Then, 700g of each of the above roasted soil balls was added with sodium silicate, directing agent, sodium hydroxide solution, and chemical water, and hydrothermally crystallized at 87℃ for 16h, and the mother liquor was filtered out, washed with water, and dried to obtain the product. After being calcined at 800℃ for 1h in a pretreatment furnace, 900g of a catalyst containing 40wt% Y-type molecular sieve and 0.8wt% ignition loss is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 180μm and a pressure of 5MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 30:1. The gas-solid phase reaction temperature is 600℃, and the contact time with the gas is 50min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.45:1. The inner diameters of the buffer zone and the reaction zone are 0.45m and 0.3m, respectively, and the heights are 0.7m and 0.5m, respectively. The reacted gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 10wt% sodium hydroxide solution. After the reacted material is purged in the absorption tower for 25min, the gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water. The catalyst washed with water: H2O = 1:15, pH value is 4.8, washing temperature is 75°C, and washing time is 1h. Then nitric acid is used for exchange, the exchange pH is 3, the temperature is 95°C, and the exchange time is 40min. The product after exchange is washed and dried to become cat-5.

[0116] Example 6

[0117] 7100g kaolin (burning base), 9wt% sodium pyrophosphate (100% kaolin), 9wt% silica sol (100% kaolin), chemical water were used to prepare a mixed slurry with a solid content of 38wt%, and spray dried to obtain 3500g spray soil balls with a particle size of 20-110μm. One part of the spray soil balls was roasted at 960℃ for 1.4h, and the other part was roasted at 880℃ for 2h, then 600g kaolin and 400g partial soil were added with sodium silicate, directing agent, sodium hydroxide solution, chemical water, and hydrothermal crystallization was carried out at 92℃ for 34h, the mother liquor was filtered out, and the product was washed and dried. In the pretreatment furnace, after calcination at 600℃ for 3h under 20% water vapor, 900g of catalyst containing 25wt% Y-type molecular sieve and ignition reduction of 2wt% was slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 130μm and a pressure of 2.2MPa. After spraying by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 90:1. The gas-solid phase reaction temperature is 300℃, and the contact time with the gas is 20min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.37:1. The inner diameters of the buffer zone and the reaction zone are 0.2m and 0.1m respectively, and the heights are 0.4m and 0.6m respectively. The reacted material is purged in the absorption tower for 30 minutes, and the gas is pumped out through the gas outlet pipe and enters the recovery system. The recovery system is a 5wt% sodium carbonate solution, which neutralizes and collects the reacted gas. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water. The washed catalyst: H2O=1:8, pH value is 5.8, washing temperature is 85°C, and washing time is 0.5h. Then nitric acid is used for exchange, the exchange pH is 4.0, the temperature is 95°C, and the exchange is 60min. The product after the exchange is washed and dried to become cat-6.

[0118] Example 7

[0119] 6100g kaolin (burning base), 2wt% sodium silicate (with kaolin as 100%), 3wt% aluminum sol, chemical water are prepared into a mixed slurry with a solid content of 38wt%, spray dried to obtain 3500g spray soil balls with a particle size of 20-110μm. One part of the spray soil balls is roasted at 850℃ for 1.4h, and the other part is roasted at 680℃ for 2h, then 700g kaolin and 500g partial soil are added with sodium silicate, directing agent, sodium hydroxide solution, chemical water, hydrothermally crystallized at 89℃ for 32h, the mother liquor is filtered to remove, washed with water, and dried to obtain the product. After being calcined at 660°C for 3h in a pretreatment furnace, 700g of a catalyst containing 38wt% Y-type molecular sieve and 1.6wt% ignition loss was slowly added to the top of the downward bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 70μm and a pressure of 3.5MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 60:1. The gas-solid phase reaction temperature is 800°C. The contact time with the gas is 10min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.23:1. The inner diameter of the buffer zone and the reaction zone are both 0.25m, and the heights are 0.6m and 0.9m respectively. After the reacted material is purged through the absorption tower for 20min, the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 13wt% sodium hydroxide solution, and the reacted gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water. The catalyst washed with water: H2O = 1:23, pH value is 6.8, washing temperature is 95°C, and washing time is 0.5h. Then it is exchanged with hydrochloric acid, the exchange pH is 5.2, the temperature is 80°C, and the exchange time is 30min. The product after the exchange is washed and dried to become cat-7.

[0120] Example 8

[0121] 4200g of kaolin (burning base), 8wt% of sodium silicate (100% of kaolin), 7wt% of aluminum sol and chemical water were prepared into a mixed slurry with a solid content of 42wt%, and spray dried to obtain 750g of spray soil balls with a particle size of 20-110μm. The spray soil balls were roasted at 630℃ for 2.1h, and then sodium silicate, a directing agent, a sodium hydroxide solution and chemical water were added, and hydrothermal crystallization was carried out at 94℃ for 36h, and the mother liquor was filtered out, and the product was washed and dried. The product is exchanged with rare earth chloride, rare earth chloride / product=0.06, exchanged at pH=3.0-4.5, 93°C for 1.5 hours, filtered to remove the filtrate, the filter cake is roasted at 700°C for 2 hours in a pretreatment furnace, 500 grams of catalyst containing 18wt% Y-type molecular sieve and 1.6wt% ignition reduction is slowly added to the top of the descending bed reactor through a feeder, the top of the reactor is an atomizer with an air eye diameter of 85μm and a pressure of 4.7MPa, the catalyst particles are dispersed in the reactor through the spraying of the atomizer, run downward, and meet silicon tetrachloride gas, the ratio of silicon tetrachloride to nitrogen is 50:1, the gas-solid phase reaction temperature is 700°C, the contact time with the gas is 2min, and the gas flow is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.14:1. The inner diameters of the buffer zone and the reaction zone are 0.3m and 0.15m respectively, and the heights are 0.8m and 1m respectively. After the reacted material is purged in the absorption tower for 50 minutes, the gas is pumped out through the gas outlet pipe and enters the recovery system. The recovery system is a 10wt% sodium carbonate solution, which neutralizes and collects the reacted gas. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water. The washed catalyst: H2O=1:18, pH value is 3.8, washing temperature is 65°C, and washing time is 2h. Then sulfuric acid is used for exchange, the exchange pH is 4.7, the temperature is 95°C, and the exchange is 30min. The product after the exchange is washed and dried to become cat-8.

[0122] Example 9

[0123] 2400g kaolin (calcined base), 15wt% sodium pyrophosphate (based on kaolin as 100%), 18wt% silica sol (based on kaolin as 100%), and chemical water were prepared into a mixed slurry with a solid content of 42wt%, and spray-dried to obtain 1550g of spray soil balls with a particle size of 20-110μm.

[0124] Part of the sprayed soil balls were calcined at 890°C for 1.5h, and the other part was calcined at 770°C for 1.8h. Then 200g and 400g of the above-mentioned baked soil balls were added with sodium silicate, directing agent, sodium hydroxide solution, and chemical water, and hydrothermally crystallized at 88°C for 28h. The mother liquor was filtered out, and the product was washed with water and dried. In the pretreatment furnace, the product is roasted at 550℃ for 6h, and then 800g of catalyst containing 13wt% Y-type molecular sieve and 2.5wt% ignition reduction is slowly added to the top of the downward bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 160μm and a pressure of 5.5MPa. After the spraying of the atomizer, the catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 40:1, the gas-solid phase reaction temperature is 450℃, and the contact time with the gas is 1min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to in-situ crystallization catalyst is 0.08:1. The inner diameter of the buffer zone and the reaction zone are both 0.5 meters, and the heights are 0.9 meters and 0.4 meters respectively. After the reacted material is purged in the absorption tower for 35 minutes, the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is an 8wt% sodium carbonate solution, and the reacted gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is first washed with water, the catalyst washed with water: H2O = 1:12, pH value is 7.8, washing temperature is 45°C, washing time is 2h. Then it is exchanged with phosphoric acid, the exchange pH is 5.8, the temperature is 80°C, and the exchange time is 30min. The product after the exchange is washed and dried to become cat-9.

[0125] Comparative Example 1

[0126] Compared with Example 9, the conditions in the pretreatment furnace are the same. 800 grams of catalyst containing 13wt% Y-type molecular sieve and ignition reduction of 2.5wt% are slowly added to the top of the inclined tubular reactor through a feeder, slowly fall by gravity, and meet silicon tetrachloride gas at the reactor inlet. The ratio of silicon tetrachloride to nitrogen is 40:1, the gas-solid phase reaction temperature is 450°C, and the contact time with the gas is 1min. The flow rate of the gas is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.08:1. The inner diameter of the reaction zone is 0.5 meters and the height is 1.3 meters. After the reacted material is purged by the absorption tower for 35 minutes, the gas is discharged by pumping through the gas outlet pipe and enters the recovery system. The recovery system is an 8wt% sodium carbonate solution, and the reacted gas is acid-base neutralized and collected. The catalyst after the reaction is collected by the collector at the bottom of the absorption tower and then washed with water. The catalyst after the water washing: H2O = 1:12, pH value is 7.8, washing temperature is 45°C, and washing time is 2h. Then phosphoric acid is used for exchange, the exchange pH is 5.8, the temperature is 80°C, and the exchange time is 30min. The product after the exchange is washed and dried to become cat-10.

[0127] Comparative Example 2

[0128] Compared with Example 7, 6100g of kaolin (burning base), 2wt% of sodium silicate (based on kaolin as 100%), 3wt% of aluminum sol (based on kaolin as 100%), and chemical water were prepared into a mixed slurry with a solid content of 38wt%, and spray-dried to obtain 3500g of spray-soil balls with a particle size of 20 to 110μm. A portion of the spray-soil balls was roasted at 850℃ for 1.4h, and the other portion was roasted at 680℃ for 2h, then 700g of kaolin and 500g of partial clay were added with sodium silicate, a directing agent, a sodium hydroxide solution, and chemical water, and hydrothermally crystallized at 89℃ for 32h, the mother liquor was filtered out, and the product was washed and dried. After calcination at 660°C for 3h in a pretreatment furnace, 700g of a catalyst containing 38wt% Y-type molecular sieve and 1.6wt% ignition reduction was slowly added to the interior of the kettle fixed bed reactor through a feeder. The material was stirred by stirring, and silicon tetrachloride gas was introduced. The ratio of silicon tetrachloride to nitrogen was 10:1. The gas-solid phase reaction temperature was 400°C, and the contact time with the gas was 60min. The gas flow rate was controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst was 0.3:1. The inner diameter of the reaction zone was 0.25 meters and the height was 1.5 meters. After the reacted material was absorbed by the absorption tower, the gas was pumped out through the gas outlet pipe and entered the recovery system. The recovery system was a 12wt% sodium hydroxide solution, and the reacted gas was acid-base neutralized and collected. After the catalyst was collected by the collector at the bottom of the absorption tower, it was first washed with water. The washed catalyst: H2O = 1:1, pH value was 2.5, washing temperature was 70°C, and washing time was 2.5h. Then, oxalic acid was used for exchange at a pH of 5.1, a temperature of 80°C, and a period of 30 minutes. The product after the exchange was washed and dried to obtain cat-11.

[0129] Comparative Example 3

[0130] Compared with Example 3, 1300g of kaolin (burning base), 15wt% of sodium silicate (based on kaolin as 100%), 5wt% of aluminum sol, and chemical water were prepared into a mixed slurry with a solid content of 40wt%, spray dried to obtain 600g of spray soil balls with a particle size of 20 to 110μm. The spray soil balls were roasted at 990℃ for 1.5h, sodium silicate, directing agent, sodium hydroxide solution, and chemical water were added, and hydrothermal crystallization was carried out at 85℃ for 16h, the mother liquor was filtered out, and the product was washed and dried. After being calcined at 700℃ for 2h in the pretreatment furnace, 600g of catalyst containing 40wt% Y-type molecular sieve and ignition reduction of 2.8wt% is slowly added to the top of the descending bed reactor through a feeder. The catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The ratio of silicon tetrachloride to nitrogen is 60:1, the gas-solid phase reaction temperature is 800℃, and the contact time with the gas is 10min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.23:1. The inner diameter of the reaction zone is 0.2m and the height is 0.7m. The reacted gas is pumped out through the gas outlet pipe and enters the recovery system. The recovery system is a 13wt% sodium hydroxide solution, which neutralizes and collects the reacted gas. The reacted catalyst is collected by the collector at the bottom of the absorption tower and then washed with water. The washed catalyst: H2O=1:23, pH value is 6.8, washing temperature is 95℃, and washing time is 0.5h. Then, hydrochloric acid was used for exchange at a pH of 5.2, a temperature of 80°C, and a period of 30 minutes. The product after the exchange was washed and dried to obtain cat-12.

[0131] Table 1 Gas-solid phase reaction implementation effect

[0132]

[0133] The gas-solid reaction effects of the embodiment and the comparative example are shown in Table 1. Under the same reaction conditions, only the reactor form of the gas-solid phase reaction and the catalyst feeding downward operation mode are changed, which can sensitively reflect the reduction of the sodium oxide content of the catalyst and the change of the 17-hour micro-reaction activity. The isomorphous substitution process and equipment of the present invention have a more excellent sodium oxide reduction effect and the advantage of ensuring the micro-reaction activity of the catalyst, which lays a foundation for the long-term stable operation of the catalyst on the device.

[0134] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.

Claims

1. A gas phase ultrastable reactor, characterized in that: The gas phase ultrastable reactor is divided into a buffer zone and a reaction zone from top to bottom. A catalyst inlet is provided at the top of the buffer zone, an atomizer connected to the catalyst inlet is provided at the upper part of the buffer zone, a nitrogen inlet carrying silicon tetrachloride is provided at the bottom of the reaction zone, and a discharge port is provided at the upper part of the reaction zone. The inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 4:1, the heights of the buffer zone and the reaction zone are 0.2 to 1 meter respectively, and the weight ratio of the silicon tetrachloride to the catalyst when reacting in the reaction zone is 0.01 to 0.5:

1.

2. The gas phase ultrastable reactor according to claim 1, characterized in that: The inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 3:1; a heating jacket or a heating belt is arranged on the outer wall of the gas phase ultrastable reactor; the cavity diameter of the buffer zone is 0.05 to 0.5 meters and the height is 0.2 to 1 meters.

3. The gas phase ultrastable reactor according to claim 1, characterized in that: The atomizer is made of stainless steel and contains a plurality of symmetrically distributed air holes. The diameter of the air holes is 80-200 um. The gas pressure inside the atomizer is 0.1-6 MPa.

4. A device for increasing the silicon-aluminum ratio of a catalytic cracking catalyst, characterized in that: include: A pretreatment furnace, used for calcining or hydrothermal treatment of the catalyst to obtain a pretreated catalyst; The gas phase ultrastable reactor according to any one of claims 1 to 3, used for performing isomorphous substitution reaction on the pretreated catalyst to obtain the reacted catalyst; The absorption tower is used to blow the reacted catalyst from the feed port into the absorption tower, and then the tail gas neutralization reaction occurs to obtain the catalyst intermediate; Exchange filter, used for exchange and filtration of catalyst intermediates; Flash drying equipment, used for flash evaporation and drying of catalyst intermediates.

5. The device for increasing the silicon-aluminum ratio of catalytic cracking catalyst according to claim 4, characterized in that: It also includes a recovery system for recovering nitrogen carrying silicon tetrachloride in the gas phase ultra-stable reactor.

6. The device for increasing the silicon-aluminum ratio of catalytic cracking catalyst according to claim 4, characterized in that: The pretreatment furnace comprises a feeding section, a roasting section and a discharging section. The total length of the pretreatment furnace is 0.5 to 5 meters, the inner diameter is 0.01 to 1 meter, and the roasting temperature is 100 to 1000°C.

7. The device for increasing the silicon-aluminum ratio of catalytic cracking catalyst according to claim 4, characterized in that: The pretreatment furnace includes a heating system and a ventilation system. The heating system is arranged on the outer layer of the pretreatment furnace in the form of a furnace tile jacket, and the ventilation system is arranged on the inner wall of the pretreatment furnace. The ventilation system can input dry gas, nitrogen or water vapor into the pretreatment furnace.

8. The device for increasing the silicon-aluminum ratio of catalytic cracking catalyst according to claim 4, characterized in that: The angle α between the pretreatment furnace feeding section and the pretreatment furnace body is greater than 10° and less than 90°, and the angle β between the pretreatment furnace body and the horizontal position is greater than 10° and less than 90°.

9. The device for increasing the silicon-aluminum ratio of catalytic cracking catalyst according to claim 4, characterized in that: A shaft rotating device is provided on the top of the pretreatment furnace to control the rotation of the furnace body of the pretreatment furnace, and the rotation frequency is 10 to 80 Hz / min.

10. A method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst, characterized in that: The device for improving the silicon-aluminum ratio of a catalytic cracking catalyst according to any one of claims 4 to 9 comprises the following steps: S1. The catalyst is calcined or hydrothermally treated in a pretreatment furnace to obtain a pretreated catalyst; S2, the pretreated catalyst enters a gas phase ultrastable reactor and contacts with nitrogen carrying silicon tetrachloride to undergo an isomorphous substitution reaction, wherein the weight ratio of the silicon tetrachloride to the catalyst is 0.01 to 0.5:1; S3. The catalyst after the reaction is purged, collected, and washed with water in an absorption tower, and then ammonium-free exchange, washing, and drying are performed to obtain a finished product.

11. The method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst according to claim 10, characterized in that: The following steps are also included: S4. The gas after the reaction enters a recovery system, wherein the alkaline solution in the recovery system is at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate, and the concentration of the alkaline solution is 1-20 wt%.

12. The method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst according to claim 10, characterized in that: After the catalyst passes through the pretreatment furnace, the pretreated catalyst has a ignition loss within 3wt% and a Y-type molecular sieve content of 5-60wt%.

13. The method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst according to claim 10, characterized in that: In the gas phase ultra-stable reactor, the temperature is 200-900° C., the contact time between the catalyst and the silicon tetrachloride gas is 0.1-60 min, the weight ratio of the catalyst to the silicon tetrachloride gas is 0.01-0.5:1, and the volume ratio of silicon tetrachloride to nitrogen in the nitrogen carrying silicon tetrachloride is 0.1-100:

1.

14. The method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst according to claim 10, characterized in that: The inner diameter of the absorption tower is 1 to 50 cm, and the time for passing gas to purge the material is 10 to 120 minutes.

15. The method for increasing the silicon-aluminum ratio of a catalytic cracking catalyst according to claim 10, characterized in that: The catalyst is prepared by an in-situ crystallization process.