Antibacterial polycarbonate film and preparation method thereof

By adding inorganic antibacterial agents and pigment fillers to the polycarbonate film, the antibacterial polycarbonate film with a double-layer structure has been solved, and the problems of poor antibacterial properties, large color difference and serious cross-border in the prior art have been achieved, and efficient antibacterial properties and Product quality has been improved.

CN115805733BActive Publication Date: 2024-11-05JIANGSU HANYANG NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211353551.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-01
Publication Date
2024-11-05
Estimated Expiration
2042-11-01

AI Technical Summary

Technical Problem

The existing polycarbonate films have poor antibacterial properties in applications in electronic products and medical devices, and the batch color aberration and cross-line problems caused by printing inks affect the use effect of the product.

Method used

Design of antibacterial polycarbonate film with a two-layer structure, in which the outer layer is a polycarbonate film layer with inorganic sustained release antibacterial agent, and the inner layer is a polycarbonate film layer with color, which is added to the polycarbonate resin. Nanosilver, nanozinc oxide and sustained-release fluoride ion antibacterial agents, and pigment fillers and lubricants are added during the extrusion process to avoid the use of printing layers, thereby improving antibacterial properties and reducing color aberrations.

Benefits of technology

It has achieved significant improvement in the antibacterial performance of polycarbonate films, reduced the production cost and environmental pollution of the product, reduced the occurrence of batch color difference and cross-border lines, and improved the quality and service life of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003919978390000101
    Figure BDA0003919978390000101
Patent Text Reader

Abstract

The present invention discloses an antibacterial polycarbonate film, comprising a first polycarbonate film layer and a second polycarbonate film layer, wherein the first polycarbonate film layer comprises a polycarbonate resin and an inorganic sustained-release antibacterial agent, and the second polycarbonate film layer comprises a polycarbonate resin, a pigment filler, an antioxidant, and a lubricant. The present invention also discloses a method for preparing an antibacterial polycarbonate film. The polycarbonate film is configured to include a first PC layer and a second PC layer, and the inorganic sustained-release antibacterial agent in the first PC layer enables the PC film to have better sterilization efficiency, low cost, and environmental protection without pollution. The second PC pellets are prepared by adding pigment fillers and other fillers to the PC resin, and a colored PC film is prepared by extruding through an extruder. Since there is no need to prepare a printing layer, the appearance of printing horizontal stripes is avoided, and the probability of batch product color difference caused by printing ink is also greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polycarbonate films, and in particular to an antibacterial polycarbonate film and a preparation method thereof. Background Art

[0002] Polycarbonate film has good comprehensive properties. Ordinary films are colorless and transparent, with a light transmittance of more than 90%. The film not only has excellent electrical properties, but also has high tensile strength and rigidity, and its impact resistance is also the highest among thermoplastics. The water absorption rate and product molding shrinkage rate of polycarbonate film are low, and the creep resistance is excellent. Therefore, the product size is stable under different temperature and humidity conditions, which is suitable for the production of precision components. In particular, its cold resistance and heat resistance are very excellent, and it can work for a long time in a wide range of 100℃ to 130℃.

[0003] Since polycarbonate film is transparent, non-toxic, tasteless and odorless, its printability and secondary processing performance such as metal evaporation and vacuum forming are also very good. It can be processed and replicated into various beautiful decorations, or made into various composite products with other materials. The products are mainly used in: automotive industry, electronics, electrical industry, membrane switches, nameplates, LCD screens, industrial machinery parts, mirror plating, various signs, printing, protective masks, sun hats, sunglasses and other fields.

[0004] At present, the nameplates or labels widely used in electronic products, electrical appliances and medical devices are mostly made of polycarbonate film. Due to the need for identification, this type of polycarbonate film is usually composed of a transparent polycarbonate film and a printing layer, which has the following disadvantages in use. First, the existing nameplates or labels made of polycarbonate film do not have antibacterial effects or have poor antibacterial properties, which limits their application in the fields of electronic products, household appliances and medical devices that people have more contact with in daily life; secondly, when making polycarbonate nameplates or labels, the existing technology usually prints ink on one side of the transparent polycarbonate film. Since the ink contains a large amount of organic solvents and organic matter, it is easy to pollute the environment; on the other hand, after printing ink on the surface of the polycarbonate film, it will cause large batch color differences in the products, and the surface of the products produced will have serious horizontal lines, which will affect the use effect of the products. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects in the prior art and provide an antibacterial polycarbonate film and a method for preparing the same, aiming to solve the problems of the existing polycarbonate film having poor antibacterial properties, large color differences between product batches, and severe horizontal stripes on the product surface.

[0006] To achieve the above-mentioned purpose, the technical solution of the present invention is to provide an antibacterial polycarbonate film, comprising a first polycarbonate film layer and a second polycarbonate film layer, wherein the components of the first polycarbonate film layer include polycarbonate resin and an inorganic sustained-release antibacterial agent, and the second polycarbonate film layer includes polycarbonate resin, pigment filler, antioxidant, and lubricant.

[0007] In order to make the polycarbonate film have an antibacterial effect and avoid the product batch color difference and production horizontal stripes caused by printing ink, the technical solution adopted by the present invention is to design the polycarbonate film into a two-layer structure, the outer layer is an antibacterial polycarbonate film (PC) layer, and the inner layer is a colored polycarbonate film (PC) layer. The antibacterial PC layer, that is, the first PC layer, is a sustained-release antibacterial layer, and its components include PC resin and inorganic sustained-release antibacterial agents. Compared with organic antibacterial agents, inorganic antibacterial agents have better bactericidal efficiency, and have the advantages of low cost, environmental protection and no pollution. The inner colored PC layer is prepared by adding pigment fillers and other additives to the PC resin. Since the inner layer is in direct contact with the product, adding antibacterial agents only in the outer layer can not only make the PC film have better antibacterial properties, but also reduce the amount of antibacterial agents used, thereby reducing the production cost of the product. Pigment fillers and other fillers are added to PC resin to prepare a second PC pellet, and a colored PC film is prepared by extruding it through an extruder. Since there is no need to prepare a printing layer, the probability of batch product color difference caused by printing ink is greatly reduced.

[0008] A further preferred technical solution is that, by weight percentage, the components of the first polycarbonate film layer include 95-98.5% polycarbonate resin, 0.05-0.3% nano silver, 0.5-2% nano zinc oxide, 0.5-2% sustained-release fluoride antibacterial agent, and 0.3-2% silane coupling agent. In order to make the polycarbonate film have an antibacterial effect, researchers usually add antibacterial agents to the polycarbonate resin, or make an antibacterial coating on the surface of the polycarbonate film. Making an antibacterial coating on the surface of the polycarbonate film will not only increase the production process of the product, but also greatly increase the production cost of the product. On the other hand, the coating has poor wear resistance and a short service life. After long-term use, the coating will partially or completely fall off, affecting the customer's experience. Adding an antibacterial agent to a polycarbonate resin and making a polycarbonate film is currently the most commonly used method for making an antibacterial film, and silver ion antibacterial agents are the most commonly used antibacterial agents. Although silver ion antibacterial agents have good antibacterial properties, during the process of mixing the silver ion antibacterial agent with polycarbonate resin and melt extruding at high temperature, as the temperature rises, the silver ions will gradually evaporate and the antibacterial properties of the antibacterial agent will be weakened, which greatly reduces the antibacterial properties of the final product.

[0009] In order to further improve the antibacterial properties of polycarbonate film, the technical solution further adopted by the present invention is to add an inorganic antibacterial agent to the polycarbonate resin to prepare the first PC layer, wherein the inorganic antibacterial agent includes nano silver, nano zinc oxide and a slow-release fluoride ion antibacterial agent, and the addition of the slow-release fluoride ion antibacterial agent can not only make the polycarbonate film continuously release fluoride ions during use, further improving the antibacterial properties of the product, but also the addition of fluoride ions can improve the high temperature resistance of silver ions, so that silver ions are not easy to volatilize during the melting process, and the final product will gradually release silver ions during use, playing a bactericidal and antibacterial effect. At the same time, the slow-release fluoride ion antibacterial agent has good compatibility with polycarbonate, and the slow-release fluoride ion antibacterial agent can be more evenly dispersed in the polycarbonate film. In order to further increase the dispersibility of the antibacterial agent, the components of the first PC layer also contain a silane coupling agent, and the addition of the silane coupling agent can promote the dispersion of nano silver, zinc oxide and the slow-release fluoride ion antibacterial agent.

[0010] A further preferred technical solution is that, by weight percentage, the components of the second polycarbonate film layer include 97-99% polycarbonate resin, 0.5-2.5% pigment filler, 0.05-0.1% antioxidant, and 0.15-0.5% lubricant. Preferably, the content of polycarbonate resin can be 97%, 97.5%, 98%, 98.5% or 99%, the content of pigment filler can be 0.5%, 1%, 1.5%, 2% or 2.5%, the content of antioxidant is preferably 0.05%, 0.06%, 0.07%, 0.08%, 0.09% or 0.1%, and the content of lubricant is preferably 0.15%, 0.2%, 0.3%, 0.4% or 0.5%.

[0011] A further preferred technical solution is that the sustained-release fluoride ion antibacterial agent includes a fluoride salt, and the fluoride salt includes one or a mixture of barium fluoride, sodium fluoride, and potassium fluoride.

[0012] A further preferred technical solution is that in the second polycarbonate film layer, the pigment filler includes, by weight percentage, 0.5% to 1% carbon black, 0.05% to 0.1% titanium yellow, and 0.5% to 1% titanium dioxide.

[0013] A further preferred technical solution is that the lubricant includes an internal lubricant and an external lubricant. In terms of mass percentage, the content of the internal lubricant is 0.08% to 0.1%, and the content of the external lubricant is 0.08% to 0.1%. The internal lubricant is mainly a lubricant that reduces the friction within the polymer molecular chain during polymer processing. The internal lubricant has good compatibility with the polymer and can be evenly dispersed between the molecular chains to improve the fluidity of the polymer and improve the surface finish of the product. After the external lubricant is added to polycarbonate to make a PC film, it tends to migrate to the surface of the polycarbonate film and form a lubricant molecule layer at the interface, thereby improving the surface properties of the film. The external lubricant is usually selected from some higher fatty acids and organic wax products.

[0014] The present invention also provides a method for preparing an antibacterial polycarbonate film, comprising the following steps:

[0015] (1) placing an inorganic antibacterial agent in a high-speed mixer and mixing it uniformly, and then fully and uniformly mixing it with a polycarbonate resin in a high-speed mixer, and then feeding it into a twin-screw extruder from a feeder to be melted, extruded and granulated to obtain a first polycarbonate pellet;

[0016] (2) mixing the pigment filler in a high-speed mixer, and dispersing the pigment filler with the polycarbonate resin, the antioxidant, and the lubricant by ultrasonic wave, and after being fully and evenly mixed, the pigment filler is fed into a twin-screw extruder from a feeder to be melted, extruded and granulated to obtain a second polycarbonate pellet;

[0017] (3) respectively placing the first polycarbonate pellets and the second polycarbonate pellets into a vacuum dryer for drying;

[0018] (4) The fully dried first polycarbonate pellets and the second polycarbonate pellets are introduced into an extruder respectively, and the molten blend is melt-extruded through a T-die; the melt flowing out of the T-die is rolled and shaped by a steel roller and a rubber roller, and then a polycarbonate film is drawn out.

[0019] A further preferred technical solution is that in step (1) and step (2), the temperature during melt granulation is 180-230°C.

[0020] A further preferred technical solution is that in step (2), the ultrasonic frequency is 20-40KHz, the dispersion speed is 5000-8000r / min, and the dispersion time is 30-60min; in order to improve the large batch color difference of the product and the horizontal lines on the surface of the product, in addition to improving the structure of the product and removing the printing process, another major improvement is that after the molten pellets are extruded through the die head, they are calendered and shaped by a steel roller on one side and a rubber roller on the other side. In the actual production of products, it was found that when the polycarbonate film is thick, if the calendering is carried out using a device with steel rollers on both sides, horizontal lines will be left on the surface of the polycarbonate film. If a device with a rubber roller on one side and a steel roller on the other side is used for calendering and shaping, the appearance of horizontal lines can be effectively reduced, further improving the quality of the product.

[0021] The advantages and beneficial effects of the present invention are:

[0022] 1. The polycarbonate film is set to a structure including a first PC layer and a second PC layer. The inorganic slow-release antibacterial agent in the first PC layer makes the PC film have better sterilization efficiency, low cost, environmental protection and no pollution. The second PC pellets are prepared by adding pigment fillers and other fillers to the PC resin, and the colored PC film is prepared by extrusion through an extruder. Since there is no need to prepare a printing layer, the appearance of printing stripes is avoided, and the probability of batch product color difference caused by printing ink is greatly reduced.

[0023] 2. The addition of the slow-release fluoride antibacterial agent can not only make the polycarbonate film continuously release fluoride ions during use, further improving the antibacterial properties of the product, but also improve the high temperature resistance of silver ions, making it difficult for silver ions to volatilize during the melting process. The final product will gradually release silver ions during use, playing a role in sterilization and inhibition of bacteria. At the same time, the slow-release fluoride antibacterial agent has good compatibility with polycarbonate and can be evenly dispersed in the polycarbonate film.

[0024] 3. After the molten pellets are extruded through the die head, they are calendered and shaped by a steel roller on one side and a rubber roller on the other side, which can effectively reduce the appearance of horizontal lines and further improve the quality of the product. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is further described below in conjunction with the examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and cannot be used to limit the protection scope of the present invention.

[0026] Example 1

[0027] An antibacterial polycarbonate film comprises a first polycarbonate film layer and a second polycarbonate film layer. The first polycarbonate film layer comprises 95% polycarbonate resin, 0.3% nano silver, 2% nano zinc oxide, 0.7% sodium fluoride, and 2% silane coupling agent, and the second polycarbonate film layer comprises 97% polycarbonate resin, 1% carbon black, 0.1% titanium yellow, 1.5% titanium dioxide, 0.1% antioxidant, 0.1% internal lubricant, and 0.2% external lubricant.

[0028] A method for preparing an antibacterial polycarbonate film comprises the following steps:

[0029] (1) placing an inorganic antibacterial agent in a high-speed mixer and mixing it, and then mixing it with a polycarbonate resin in a high-speed mixer and then feeding it into a twin-screw extruder from a feeder to melt at a melting temperature of 180° C., and then extruding and granulating the melted polycarbonate to obtain a first polycarbonate pellet;

[0030] (2) mixing the pigment filler in a high-speed stirrer, and dispersing the pigment filler with the polycarbonate resin, the antioxidant, and the lubricant by ultrasonic wave, and after being fully and evenly mixed, the pigment filler enters a twin-screw extruder from a feeder for melting, and is extruded into granules to obtain a second polycarbonate granule. The ultrasonic wave frequency is 20 kHz, the dispersion speed is 5000 r / min, the dispersion time is 30 min, and the temperature during the melt granulation is 180° C.;

[0031] (3) respectively placing the first polycarbonate pellets and the second polycarbonate pellets into a vacuum dryer for drying;

[0032] (4) The fully dried first polycarbonate pellets and the second polycarbonate pellets are introduced into an extruder respectively, and the molten blend is melt-extruded through a T-die at a temperature of 200° C. The melt flowing out of the T-die is rolled and shaped by a steel roller and a rubber roller, and then a polycarbonate film is drawn out.

[0033] Example 2

[0034] An antibacterial polycarbonate film comprises a first polycarbonate film layer and a second polycarbonate film layer. The first polycarbonate film layer comprises 96% polycarbonate resin, 0.05% nano silver, 2% nano zinc oxide, 0.5% sodium fluoride, and 1.45% silane coupling agent, in terms of mass percentage. The second polycarbonate film layer comprises 99% polycarbonate resin, 0.2% carbon black, 0.06% titanium yellow, 0.5% titanium dioxide, 0.06% antioxidant, 0.06% internal lubricant, and 0.08% external lubricant.

[0035] A method for preparing an antibacterial polycarbonate film comprises the following steps:

[0036] (1) putting an inorganic antibacterial agent into a high-speed mixer and mixing it, and then mixing it with a polycarbonate resin in a high-speed mixer and then feeding it into a twin-screw extruder from a feeder to melt at a temperature of 200° C. After melting, extrusion and granulation are performed to obtain a first polycarbonate pellet;

[0037] (2) mixing the pigment filler in a high-speed stirrer, and dispersing the pigment filler with the polycarbonate resin, antioxidant, and lubricant by ultrasonic wave, and after being fully and evenly mixed, the pigment filler enters a twin-screw extruder from a feeder for melting, extrusion granulation, and obtains a second polycarbonate pellet. The ultrasonic wave frequency is 30 KHz, the dispersion speed is 6000 r / min, the dispersion time is 50 min, and the temperature during melt granulation is 200° C.;

[0038] (3) respectively placing the first polycarbonate pellets and the second polycarbonate pellets into a vacuum dryer for drying;

[0039] (4) The fully dried first polycarbonate pellets and the second polycarbonate pellets are introduced into an extruder respectively, and the molten blend is melt-extruded through a T-die at a temperature of 250°C; the melt flowing out of the T-die is rolled and shaped by a steel roller and a rubber roller, and then a polycarbonate film is drawn out at a certain film drawing rate.

[0040] Example 3

[0041] An antibacterial polycarbonate film comprises a first polycarbonate film layer and a second polycarbonate film layer. The first polycarbonate film layer comprises 97% polycarbonate resin, 0.2% nano silver, 0.5% nano zinc oxide, 2% slow-release sodium fluoride, and 0.3% silane coupling agent, and the second polycarbonate film layer comprises 98.24% polycarbonate resin, 0.5% carbon black, 0.05% titanium yellow, 1% titanium dioxide, 0.05% antioxidant, 0.08% internal lubricant, and 0.08% external lubricant, in terms of mass percentage.

[0042] A method for preparing an antibacterial polycarbonate film comprises the following steps:

[0043] (1) putting an inorganic antibacterial agent into a high-speed mixer and mixing it, and then mixing it with a polycarbonate resin in a high-speed mixer and then feeding it into a twin-screw extruder from a feeder to melt at a temperature of 200° C. After melting, extrusion and granulation are performed to obtain a first polycarbonate pellet;

[0044] (2) mixing the pigment filler in a high-speed stirrer, and dispersing the pigment filler with the polycarbonate resin, the antioxidant, and the lubricant by ultrasonic wave, and after being fully and evenly mixed, the pigment filler enters a twin-screw extruder from a feeder for melting, and is extruded and granulated to obtain a second polycarbonate pellet. The ultrasonic wave frequency is 40 kHz, the dispersion speed is 6000 r / min, the dispersion time is 60 min, and the temperature during the melt granulation is 200° C.;

[0045] (3) respectively placing the first polycarbonate pellets and the second polycarbonate pellets into a vacuum dryer for drying;

[0046] (4) The fully dried first polycarbonate pellets and the second polycarbonate pellets are introduced into an extruder respectively, and the molten blend is melt-extruded through a T-die at a temperature of 230° C. The melt flowing out of the T-die is rolled and shaped by a steel roller and a rubber roller, and then a polycarbonate film is drawn out at a certain film drawing rate.

[0047] Example 4

[0048] An antibacterial polycarbonate film comprises a first polycarbonate film layer and a second polycarbonate film layer. The first polycarbonate film layer comprises 98.5% polycarbonate resin, 0.08% nano silver, 0.5% nano zinc oxide, 0.6% sodium fluoride, and 0.32% silane coupling agent, and the second polycarbonate film layer comprises 98.46% polycarbonate resin, 0.6% carbon black, 0.06% titanium yellow, 0.6% titanium dioxide, 0.08% antioxidant, 0.1% internal lubricant, and 0.1% external lubricant.

[0049] A method for preparing an antibacterial polycarbonate film comprises the following steps:

[0050] (1) placing an inorganic antibacterial agent in a high-speed mixer and mixing it, and then mixing it with a polycarbonate resin in a high-speed mixer and then feeding it into a twin-screw extruder from a feeder to be melted at a temperature of 230° C., and then extruding and granulating the melted polycarbonate to obtain a first polycarbonate pellet;

[0051] (2) mixing the pigment filler in a high-speed stirrer, and dispersing the pigment filler with the polycarbonate resin, the antioxidant, and the lubricant by ultrasonic wave, and after being fully and evenly mixed, the pigment filler enters a twin-screw extruder from a feeder for melting, and is extruded into granules to obtain a second polycarbonate granule. The ultrasonic wave frequency is 30 kHz, the dispersion speed is 8000 r / min, the dispersion time is 30 min, and the temperature during the melt granulation is 230° C.;

[0052] (3) respectively placing the first polycarbonate pellets and the second polycarbonate pellets into a vacuum dryer for drying;

[0053] (4) The fully dried first polycarbonate pellets and the second polycarbonate pellets are introduced into an extruder respectively, and the molten blend is melt-extruded through a T-die at a temperature of 280°C; the melt flowing out of the T-die is rolled and shaped by a steel roller and a rubber roller, and then a polycarbonate film is drawn out at a certain film drawing rate.

[0054] Comparative Example 1

[0055] A polycarbonate film comprises a polycarbonate film layer and an ink layer. Calculated by mass percentage, the components of the polycarbonate film layer include 98.7% polycarbonate resin, 1% titanium dioxide, 0.1% antioxidant, 0.1% internal lubricant, and 0.1% external lubricant.

[0056] A method for preparing a polycarbonate film comprises the following steps:

[0057] (1) titanium dioxide, an antioxidant, an internal lubricant and an external lubricant are mixed in a high-speed mixer, and then mixed with a polycarbonate resin by a high-speed mixer and then fed into a twin-screw extruder from a feeder for melt extrusion granulation to obtain polycarbonate pellets, and the melt extrusion temperature is 200° C.;

[0058] (2) placing the polycarbonate pellets into a vacuum dryer for drying;

[0059] (3) introducing the fully dried polycarbonate pellets into an extruder, and the molten blend is melt-extruded through a T-die; the melt flowing out of the T-die is rolled and shaped by two steel rollers to form a polycarbonate film;

[0060] (4) Printing black-gray ink on one side of the polycarbonate film obtained in step (3) and drying the film.

[0061] The polycarbonate films prepared in Examples 1 to 4 and Comparative Example 1 were taken, and their chromaticity values ​​were tested using a colorimeter, the color difference value ΔE was recorded, the horizontal lines on the film surface were observed, and the antibacterial properties were tested according to standard QB / T 2591 2003. The test results are shown in the table below.

[0062]

[0063] It can be seen from the data in the table that the polycarbonate film of the present invention not only has a high antibacterial rate, which can kill more than 98% of Staphylococcus aureus and Escherichia coli, but also has almost no color difference among products of the same batch, and only a few products have very slight horizontal lines on their surfaces.

[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An antibacterial polycarbonate film, characterized in that: It comprises a first polycarbonate film layer and a second polycarbonate film layer, wherein the first polycarbonate film layer comprises a polycarbonate resin and an inorganic sustained-release antibacterial agent, and the second polycarbonate film layer comprises a polycarbonate resin, a pigment filler, an antioxidant, and a lubricant; The components of the first polycarbonate film layer include 95-98.5% polycarbonate resin, 0.05-0.3% nano silver, 0.5-2% nano zinc oxide, 0.5-2% slow-release fluoride antibacterial agent, and 0.3-2% silane coupling agent; The second polycarbonate film layer comprises 97-99% polycarbonate resin, 0.5-2.5% pigment filler, 0.05-0.1% antioxidant, and 0.15-0.5% lubricant; The inorganic sustained-release antibacterial agent includes fluoride salts, and the fluoride salts include one or a mixture of barium fluoride, sodium fluoride and potassium fluoride.

2. The polycarbonate film according to claim 1, characterized in that In the second polycarbonate film layer, the pigment filler includes 0.5% to 1% carbon black, 0.05% to 0.1% titanium yellow, and 0.5% to 1% titanium dioxide in terms of mass percentage.

3. The polycarbonate film according to claim 1, characterized in that The lubricant includes an internal lubricant and an external lubricant. Calculated by mass percentage, the content of the internal lubricant is 0.08%-0.1%, and the content of the external lubricant is 0.08%-0.1%.

4. A method for preparing an antibacterial polycarbonate film as claimed in claim 1, characterized in that: The following steps are involved: (1) The inorganic antibacterial agent is put into a high-speed mixer and mixed evenly, and the inorganic antibacterial agent is mixed evenly with the polycarbonate resin by the high-speed mixer, and then fed into a twin-screw extruder from a feeder to be melted, extruded and granulated to obtain a first polycarbonate pellet; (2) mixing the pigment filler in a high-speed mixer, and dispersing the pigment filler with the polycarbonate resin, the antioxidant, and the lubricant by ultrasonic wave, and after being fully and evenly mixed, the pigment filler is fed into a twin-screw extruder from a feeder to be melted, extruded and granulated to obtain a second polycarbonate pellet; (3) respectively placing the first polycarbonate pellets and the second polycarbonate pellets into a vacuum dryer for drying; (4) The fully dried first polycarbonate pellets and the second polycarbonate pellets are introduced into an extruder respectively, and the molten blend is melt-extruded through a T-die; the melt flowing out of the T-die is rolled and shaped by a steel roller and a rubber roller, and then a polycarbonate film is drawn out.

5. The preparation method according to claim 4, characterized in that: In step (1) and step (2), the temperature during melt granulation is 180 to 230°C.

6. The preparation method according to claim 4, characterized in that: In step (2), the ultrasonic frequency is 20-40 kHz, the dispersion speed is 5000-8000 r / min, and the dispersion time is 30-60 min.