A method for preparing ferric phosphate using iron-containing waste

Through the liquid-liquid reaction of the solution containing ferric chloride and calcium dihydrogen phosphate after acidolysis treatment, the problem of metathesis of ferric iron and phosphate in the existing technology is solved, the preparation of high-purity ferric phosphate is achieved, the process flow is simplified and the cost is reduced. cost.

CN115806279BActive Publication Date: 2024-10-11GUIZHOU CHANHEN CHEM CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202111080723.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-15
Publication Date
2024-10-11
Estimated Expiration
2041-09-15

AI Technical Summary

Technical Problem

It is difficult to effectively utilize iron-containing waste materials to prepare high-purity, low-impurity iron phosphate with existing technology. In particular, the metathesis reaction between ferric iron and phosphate is difficult to achieve, and impurity ions affect the purity of the product.

Method used

The ferric chloride-containing mixed solution obtained by acidolysis is reacted with a calcium dihydrogen phosphate solution for a liquid-liquid reaction. By controlling the pH value and molar ratio, a metathesis reaction without purification of ferric ions is achieved to prepare high-quality ferric phosphate.

Benefits of technology

Iron phosphate with low impurity content and good morphology can be obtained without complicated impurity removal processes, which simplifies the preparation process, reduces production costs, and reduces waste liquid emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115806279B_ABST
    Figure CN115806279B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing ferric phosphate by using iron-containing waste, comprising the following steps: step a), providing a ferric chloride mixed solution obtained by acid hydrolysis of the iron-containing waste; step b), using an alkaline compound and water to adjust the pH value of the ferric chloride mixed solution to meet 0<pH≤2, Fe 3+ The concentration is 10-80 g / L to obtain an iron source solution; step c), the iron source solution described in step b) and the calcium dihydrogen phosphate solution are mixed and reacted according to the molar ratio of P to Fe of 1:1-1.8 to obtain a slurry with a pH value of 0.2-2; step d), the slurry is aged and crystallized to obtain iron phosphate. The present invention adopts a liquid-liquid reaction system of iron salt and calcium dihydrogen phosphate with high impurity content and easy hydrolysis, and shields the influence of impurity ions through multi-stage process control, so that battery-grade iron phosphate with high purity and good product quality can be obtained without deep purification of the raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste material utilization, in particular to a method for preparing ferric phosphate by utilizing iron-containing waste materials. Background Art

[0002] In recent years, with the rapid development of new energy vehicles, the demand for power lithium-ion batteries has continued to increase. Lithium iron phosphate has an olivine structure, is stable and reliable, and has a long cycle life. It has become the first choice for new energy electric commercial vehicle power supply, energy storage power station, etc. At present, most domestic lithium iron manufacturers use iron phosphate as raw material to prepare lithium iron phosphate. 4 Also known as ferric orthophosphate, the iron is trivalent, mostly in the form of dihydrate. It is difficult to dissolve in other acids except sulfuric acid, and is almost insoluble in water, acetic acid, and alcohol. LiFePO 4 Due to its high safety, long cycle life, environmental friendliness and low cost, FePO is the most promising cathode material for lithium-ion batteries. 4 As its precursor, it has the characteristics of non-toxicity, low cost and stable structure, and has also become the focus of attention.

[0003] At present, the main methods for preparing ferric phosphate are co-precipitation and hydrothermal method. Co-precipitation refers to the solution containing two or more cations, which exist in the solution in a homogeneous form. After adding a precipitant and precipitation reaction, a uniform precipitation of various components can be obtained. This method is to prepare FePO 4 The traditional method is as follows: after the iron source and the phosphorus source are dissolved, other compounds are added to precipitate, and then the product is obtained by washing, drying and calcining. The hydrothermal method is a wet chemical method that occurs in a high-pressure reactor. The external environment is high temperature and high pressure, so insoluble substances can be dissolved and recrystallized in the reaction system. From the perspective of raw materials, the preparation process of commercially available iron phosphate is mostly to make metallic iron into iron salts and then make the iron salts into iron hydroxides, to react the iron hydroxide with phosphoric acid to prepare iron phosphate, or to prepare iron phosphate by double decomposition of iron salts and phosphates.

[0004] Patent CN109928375A discloses a method for producing phosphoric acid by using a divalent iron source and a wet process. 2 PO 4 ) 2 A method for preparing ferric phosphate, in which calcium dihydrogen phosphate powder is mixed with a ferrous ion solution to obtain a solid-liquid mixed phase. In the solid-liquid reaction system, since the precipitated ferric phosphate is also solid, it is easy to adhere to the remaining solid phase, resulting in a high content of impurity calcium in the ferric phosphate. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing ferric phosphate using iron-containing waste. The method provided by the present invention can prepare ferric phosphate with low impurity content and good morphology without complicated impurity removal process.

[0006] In the prior art, ferrous iron and phosphorus sources are generally used to synthesize battery-grade ferric phosphate. There are few reports on the direct double decomposition reaction of trivalent iron and phosphate. This may be because trivalent iron is easily hydrolyzed. In order to prevent hydrolysis, the acidity has to be increased. When the acidity in the solution increases, the concentration of phosphate is low because phosphate will be converted into H 3 PO 4 , so it is difficult to obtain iron phosphate precipitation. In addition, when iron-containing waste is used as raw material to prepare iron phosphate, impurity ions will also affect whether iron phosphate can be prepared and its purity. The inventor found in the research process that when iron phosphate is prepared by using impure trivalent iron ion solution and calcium phosphate solution, not only can iron phosphate be prepared by process control, but also high-quality iron phosphate can be obtained without purifying impurities in the trivalent iron ion solution.

[0007] The present invention provides a method for preparing ferric phosphate using iron-containing waste, comprising the following steps:

[0008] Step a), providing a mixed solution containing ferric chloride obtained by acid hydrolysis of iron-containing waste;

[0009] Step b), using alkaline compounds and water to adjust the pH value of the ferric chloride mixed solution to meet 0<pH≤2, Fe 3+ The concentration is adjusted to 10-80 g / L to obtain an iron source solution;

[0010] Step c), mixing the iron source solution and the calcium dihydrogen phosphate solution described in step b) at a molar ratio of P to Fe of 1:1 to 1.8 to obtain a slurry with a pH value of 0.2 to 2;

[0011] Step d), aging and crystallizing the slurry to obtain iron phosphate.

[0012] The present invention uses a ferric chloride solution obtained by acid hydrolysis of iron-containing waste as a raw material, and performs an "over-alkali" treatment on the solution, that is, an alkaline compound is used to neutralize excess HCl, and the pH value is adjusted to be greater than 0 and less than or equal to 2, and the iron ion concentration is 10-80 g / L. It does not need to undergo extraction, precipitation and other impurity removal treatments, and can be directly used as an iron source for synthesizing iron phosphate, and undergoes a liquid-liquid reaction with a calcium dihydrogen phosphate solution to obtain high-quality iron phosphate.

[0013] In one embodiment, the ferric chloride-containing mixed solution is obtained by acid hydrolysis of ferrous waste, and the ferric chloride-containing mixed solution includes: Fe 3+ , Cl- In addition, it also includes impurity ions; the type and content of the impurity ions are related to the source of the iron-containing waste.

[0014] In order not to affect the quality of subsequent iron phosphate, in one embodiment, the impurity ions include but are not limited to Mn 2 + 、Ni 2+ , K + 、Na + Mg 2+ , Cu 2+ 、Zn 2+ 、Al 3+ and Ca 2+ In one embodiment, the impurity ions include Mn 2+ 、Ni 2+ , K + 、Na + Mg 2+ , Cu 2+ 、Zn 2+ and Al 3+ .

[0015] Specifically, the mixed solution containing ferric chloride in step a) includes: 100-200 g / L of Fe 3+ ; 200~500g / L Cl - and impurity ions; the impurity ions include less than 2000ppm of Mn 2+ ; Ni below 500ppm 2+ ; K below 2000ppm + ; Na below 2000ppm + ; Mg below 2000ppm 2+ ; Cu below 500ppm 2+ ; Zn below 500ppm 2+ ; Al below 500ppm 3+ One or more of .

[0016] Preferably, the mixed solution containing ferric chloride in step a) comprises: 100-200 g / L of Fe 3+ ; 200~500g / L Cl - and impurity ions; the impurity ions include less than 1000ppm of Mn 2+ ; Ni below 300ppm 2+ ; K below 1000ppm + ; Na below 1000ppm + ; Mg below 1000ppm 2+ ; Cu below 300ppm2+ ; Zn below 300ppm 2+ ; Al below 300ppm 3+ One or more of .

[0017] In one embodiment, the iron-containing waste is selected from ferrophosphorus, waste iron slag, pyrite cinder, red iron oxide waste or iron-containing chemical sludge.

[0018] Ferrophosphorus is an alloy formed by phosphorus and iron, which can be a mineral or its smelting product, or a by-product of phosphorus chemical industry and silicate chemical industry such as yellow phosphorus or calcium magnesium phosphate fertilizer. The electric furnace phosphorus production process will produce yellow phosphorus by-product ferrophosphorus, in which the Fe content is about 70% and the P content is about 18-26%. When ferrophosphorus is used as a raw material, the ferrophosphorus is subjected to acid hydrolysis to obtain a mixed solution containing ferric chloride. The specific treatment method can be: dissolving the ferrophosphorus in hydrochloric acid to obtain ferrous chloride, and then oxidizing the ferrous ions in the acid solution to ferric ions; or dissolving the ferrophosphorus in hydrochloric acid and introducing an oxidizing gas at the same time to obtain a ferric chloride solution.

[0019] Waste iron slag can also be used as a raw material to prepare a mixed solution containing ferric chloride. The waste iron slag is subjected to acid hydrolysis treatment to obtain a mixed solution containing ferric chloride. The specific treatment method can be: dissolving the waste iron slag in hydrochloric acid to obtain ferrous chloride, and then oxidizing the ferrous ions in the acid solution to ferric ions; or dissolving iron-containing metal waste in hydrochloric acid and simultaneously introducing an oxidizing gas to obtain a ferric chloride solution.

[0020] Pyrite slag is the slag produced in the process of pyrite acid production, which contains a large amount of iron, mainly Fe 2 O 3 In addition, it also contains SiO 2 、CaO、MgO、Al 2 O 3 For example, a typical pyrite slag composition is: about 90% Fe 2 O 3 , about 5% SiO 2 , about 1% CaO, about 1% MgO, about 1% Al 2 O 3 And about 2% of other impurities.

[0021] When pyrite cinder is used as raw material, the pyrite cinder is treated to obtain a mixed solution containing ferric chloride. The specific treatment method can be: leaching the pyrite cinder with hydrochloric acid to obtain Fe 2 O 3 Dissolve, iron ions are leached out, and a mixed solution containing ferric chloride and other impurities is obtained:

[0022] Fe 2 O 3 +6HCl=2FeCl3 +3H 2 O.

[0023] In other embodiments, the pyrite slag contains Fe 2 O 3 , including Fe 3 O 4 When FeO and FeO are present, hydrochloric acid can be used to leach out the ferric ions and ferrous ions, and then the ferrous ions are oxidized to ferric ions. A specific method for oxidizing ferrous ions to ferric ions is to pass hydrogen peroxide into the hydrochloric acid leaching solution.

[0024] Red iron oxide waste mainly comes from steel mills. Its main component is iron oxide, and also includes Ni, Mn, Zn, Cr, etc.

[0025] When red iron oxide waste or pickled red iron oxide is used as raw material, the red iron oxide waste is treated to obtain a mixed solution containing ferric chloride. The specific treatment method can be: using hydrochloric acid to leach the red iron oxide waste, Fe 2 O 3 Dissolve, leach iron ions, and obtain a mixed solution containing ferric chloride and other impurities. Iron-containing chemical sludge is pickling sludge in the production process of the metal surface treatment industry, containing Fe, lead, zinc, etc. When iron-containing chemical sludge is used as raw material, the iron-containing chemical sludge is treated to obtain a mixed solution containing ferric chloride. The specific treatment method can be: acid leach the iron-containing chemical sludge with hydrochloric acid to obtain a solution containing ferrous ions, and then oxidize the ferrous ions to ferric ions.

[0026] The present invention uses the above-mentioned iron-containing waste as raw material, uses hydrochloric acid to acid-hydrolyze it, and optionally performs oxidation treatment to obtain a ferric chloride mixed solution containing the above-mentioned impurity ions, without the need for other impurity removal treatment.

[0027] After obtaining the mixed solution containing ferric chloride, the pH value and concentration thereof are adjusted by using an alkaline compound and water, so that the pH value is greater than 0 and less than or equal to 2, and the iron ion concentration is 10 to 80 g / L. The alkaline compound can neutralize the free HCl in the mixed solution containing ferric chloride, and provide OH - , forming an over-alkaline condition, providing the necessary conditions for the subsequent formation of iron phosphate. In one embodiment, the pH value of the ferric chloride mixed solution is adjusted to 0.5-2, and the iron ion concentration is adjusted to 15-75 g / L.

[0028] In one embodiment, the alkaline compound is selected from calcium-containing alkaline compounds, sodium-containing alkaline compounds, potassium-containing alkaline compounds, etc., preferably calcium-containing alkaline compounds, and the calcium-containing alkaline compounds include lime milk, lime or limestone. Among them, lime milk, also known as slaked lime, lime water, and slaked lime, is a suspension of calcium hydroxide generated by adding calcium oxide to water, and its main component is calcium hydroxide; lime, also known as quicklime, its main component is calcium oxide; limestone is mainly composed of calcium carbonate. In one embodiment, the calcium-containing alkaline compound is selected from lime milk. In one embodiment, the concentration of the lime milk is 10-15%.

[0029] After the iron source solution is obtained in step b) of the present invention, it does not need to be further purified and can be directly used for the subsequent preparation of ferric phosphate. The iron source solution includes: 10-80 g / L Fe 3+ ; 25~200g / L Cl - and impurity ions; the impurity ions include less than 500ppm of Mn 2+ ; Ni below 200ppm 2+ ; K below 500ppm + ; Na below 500ppm + ; Mg below 500ppm 2+ ; Cu below 200ppm 2+ ; Zn below 200ppm 2+ ; Al below 200ppm 3+ One or more of .

[0030] Specifically, in one embodiment, the iron source solution includes: 10-80 g / L Fe 3+ ; 25~200g / L Cl - and impurity ions; the impurity ions include less than 100ppm of Mn 2+ ; Ni below 50ppm 2+ ; K below 100ppm + ; Na below 100ppm + ; Mg below 200ppm 2+ ; Cu below 50ppm 2+ ; Zn below 100ppm 2+ ; Al below 200ppm 3+ One or more of .

[0031] The present application uses calcium dihydrogen phosphate solution as the phosphorus source solution. In one embodiment, the pH value of the calcium dihydrogen phosphate solution is 2.5-3.0. 2 O 5 With F - The molar ratio is ≥250.

[0032] In one embodiment, the monocalcium phosphate solution can be obtained by wet-process phosphoric acid. For example, the monocalcium phosphate is obtained by mixing wet-process phosphoric acid with a calcium-containing alkaline compound to obtain the monocalcium phosphate solution.

[0033] In the process of preparing monocalcium phosphate, the calcium-containing alkaline compound is selected from any one or more of lime, lime milk, limestone, calcium phosphate or phosphate rock, preferably lime milk.

[0034] After obtaining the iron source solution and the calcium dihydrogen phosphate solution, they are mixed according to the molar ratio of P to Fe of 1:1 to 1.8 to perform double decomposition reaction:

[0035] 2FeCl 3 +Ca(H 2 PO 4 ) 2 =2FePO 4 ·2H 2 O+CaCl 2 +4HCl

[0036] In one embodiment, the temperature of the double decomposition reaction is 60-70° C., and the time is 0.5-2 hours. After the reaction is completed, the pH value of the obtained slurry is 0.2-2.

[0037] The inventors surprisingly found that by using a highly impure mixed solution containing ferric chloride and other impurities as an iron source and a monocalcium phosphate solution as a phosphorus source for a liquid phase reaction, first adjusting the highly impure mixed solution with an alkaline compound and water so that its pH value satisfies 0<pH≤2 and the iron ion concentration is 10-80 g / L, and then mixing and reacting with a molar ratio of P to Fe of 1:1-1.8, the impurity ions therein will not precipitate into the product along with the iron phosphate, and spherical iron phosphate particles with high purity, few impurity ions and good morphology consistency can be obtained, and the iron phosphate particles have no obvious agglomeration phenomenon.

[0038] After the double decomposition reaction is completed, the obtained slurry is aged and crystallized. In one embodiment, the temperature of the aging and crystallization is 80 to 99° C., and the time is 2 to 4 hours.

[0039] The slurry after aging and crystallization is subjected to solid-liquid separation, and the obtained solid is washed. The washing method can be online washing and pulping washing, so as to obtain ferric phosphate dihydrate.

[0040] In one embodiment, the washed ferric phosphate dihydrate may be dried and calcined to obtain anhydrous ferric phosphate.

[0041] In one embodiment, after the solid-liquid separation, the method further comprises:

[0042] The mother liquor obtained after the solid-liquid separation in step d) is mixed with an alkaline compound for reaction to obtain white fertilizer.

[0043] After solid-liquid separation, the mother liquor contains a large amount of calcium chloride and hydrochloric acid, which are mixed with alkaline compounds to react to obtain by-product white fertilizer, thereby reducing the generation of waste liquid.

[0044] In one embodiment, the specific process of preparing white fertilizer may be:

[0045] Add an alkaline compound to the mother liquor, adjust the pH value to 6-12, and filter and separate to obtain calcium hydrogen phosphate, i.e., white fertilizer, and the second filtrate.

[0046] The alkaline compound contains a calcium alkaline compound, a sodium alkaline compound or a potassium alkaline compound, preferably a calcium alkaline compound, such as lime or calcium carbonate. The present invention has no special restrictions on the above specific process, and those skilled in the art can adjust the parameters according to the properties of the mother liquor.

[0047] In one embodiment, obtaining white fertilizer further comprises:

[0048] The liquid obtained after separating the white fertilizer is mixed with sulfuric acid to react and obtain white gypsum.

[0049] In the present invention, after obtaining white fertilizer according to the method described above, the method further comprises:

[0050] The liquid obtained after separating the white fertilizer is mixed with sulfuric acid to react to obtain white gypsum and hydrochloric acid.

[0051] In one embodiment, after obtaining the white gypsum, the method further comprises:

[0052] The hydrochloric acid obtained after separating the white gypsum is recycled.

[0053] Specifically, the hydrochloric acid can be used to acid dissolve iron-containing waste.

[0054] See also Figure 1 , Figure 1 A typical process flow chart for preparing ferric phosphate using iron-containing waste provided in an embodiment of the present invention, using iron-containing waste, such as pyrite slag as a raw material, firstly acid-lyzing it with hydrochloric acid to obtain a ferric chloride solution and waste slag; then pre-adjusting the obtained ferric chloride solution with an alkaline compound, such as lime milk and water, so that the pH value of the obtained iron source solution is 0-2, and the iron ion concentration is 10-80 g / L; phosphoric acid, such as defluorinated wet-process phosphoric acid, is reacted with a calcium-containing alkaline compound, such as calcium carbonate or calcium oxide, to obtain a monocalcium phosphate solution, and the pH value of the monocalcium phosphate solution is controlled to be 2.5-3.0, P 2 O 5 With F -The molar ratio of the iron source solution to the calcium dihydrogen phosphate solution is ≥250; then the iron source solution and the calcium dihydrogen phosphate solution are mixed and reacted according to the molar ratio of P to Fe of 1:1 to 1.8 to obtain a slurry with a pH value of 0.2 to 2; the obtained slurry is aged and crystallized, and the solid-liquid separation is performed to obtain a crude iron phosphate. The crude iron phosphate is washed, dried and calcined to obtain a high-purity iron phosphate with a low impurity ion content. The liquid obtained by solid-liquid separation is CaCl 2 solution, adding alkaline compounds such as lime milk, adjusting the pH value to 6-12, filtering to obtain solid white fertilizer and filtrate; adding sulfuric acid to the filtrate, after solid-liquid separation, the obtained liquid is hydrochloric acid, which can be reused in the acid hydrolysis process of iron-containing waste; the obtained solid is white gypsum.

[0055] In the existing technology of preparing ferric phosphate using calcium dihydrogen phosphate and an iron source, ferrous ions and calcium dihydrogen phosphate are basically used to react. The ferrous ions are first reacted with phosphate ions to obtain ferrous dihydrogen phosphate (Fe(H 2 PO 4 ) 2 ), and then add an oxidant to oxidize and directly prepare iron phosphate precipitation, so that the product is separated and precipitated from the mixed system.

[0056] The present invention uses trivalent iron ions and phosphate solution in a hydrochloric acid system for liquid phase reaction, and utilizes the good solubility of chloride ion salts in the hydrochloric acid system to reduce the content of other impurity ions in the solid phase iron phosphate product. The present invention adopts a liquid-liquid reaction system of trivalent iron ion salts and calcium dihydrogen phosphate with high impurity content and easy hydrolysis, and shields the influence of impurity ions through multi-stage process control, so that battery-grade iron phosphate with high purity and good product quality can be obtained without deep purification of the raw materials. The process design idea of ​​the present invention is different from the existing production route of pure iron sources, and is also different from the reaction system of preparing iron phosphate with ferrous ion sources. Moreover, calcium reagents are preferably used in the process steps to avoid the introduction of sodium ions and potassium ions, and the sodium and potassium content in the product is significantly lower than that of existing commercially available products.

[0057] In the process of preparing ferric phosphate from iron-containing waste provided by the present invention, firstly, the iron-containing waste is used as a raw material, and hydrochloric acid is used to prepare a solution containing trivalent iron ions from the iron-containing waste, which is used as an iron source to carry out a liquid-liquid reaction with a calcium dihydrogen phosphate solution, thereby developing a reaction system different from the existing ferrous ion source and phosphorus source, and reducing the production cost of the ferric phosphate; at the same time, the impurity ions in the raw material are well shielded through process control, and high-purity ferric phosphate can be prepared without extraction, precipitation and other impurity removal and purification treatments, thereby simplifying the preparation process and improving production efficiency; thirdly, white fertilizer and gypsum are by-produced while preparing the ferric phosphate, and the generated hydrochloric acid is recycled, thereby reducing the discharge of wastewater and waste liquid in the preparation process, reducing costs and reducing damage to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 A typical process flow chart for preparing ferric phosphate using iron-containing waste provided in an embodiment of the present invention;

[0059] Figure 2 This is a scanning electron microscope photograph of the iron phosphate prepared in Example 3 at a scale of 2 μm;

[0060] Figure 3 This is a scanning electron microscope photograph of the iron phosphate prepared in Example 3 at a scale of 20 μm;

[0061] Figure 4 This is a scanning electron microscope photograph of the iron phosphate prepared in Comparative Example 2;

[0062] Figure 5 This is an electron microscope photo of a commercially available iron phosphate product. DETAILED DESCRIPTION

[0063] The method for preparing ferric phosphate using iron-containing waste provided by the present invention is further described below with reference to examples.

[0064] The composition of the pyrite slag used in the following examples is shown in Table 1, which is a table of raw material compositions used in the examples and comparative examples of the present invention.

[0065] Table 1 Raw material composition table of the present invention examples and comparative examples

[0066]

[0067]

[0068] Example 1

[0069] Preparation of Fe salt: hydrolyze pyrite slag with hydrochloric acid to obtain an acid solution, the composition of which is shown in Table 1; add 12% lime milk solution to the acid solution to neutralize excess HCl, then add water to adjust the pH value to 2 and the iron ion concentration to 10 g / L to obtain an iron source solution, the composition of which is shown in Table 1;

[0070] Preparation of P salt: Mix wet phosphoric acid with calcium carbonate and calcium oxide for neutralization, and separate impurities to obtain P 2 O 5 / F of the solution is 250, add pure water to adjust the pH value to 2.61 and the P concentration to 32g / L.

[0071] The Fe salt and the P salt were synthesized at a ratio of n P / Fe = 1.05, the synthesis temperature was 60°C, the synthesis time was 0.5h, the aging temperature was 90°C, the aging crystallization time was 4h, and the pH of the synthesis mother liquor was 2. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0072] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH value to 8 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of pyrite slag.

[0073] Example 2

[0074] Preparation of Fe salt: hydrolyze pyrite slag with hydrochloric acid to obtain an acid solution, the composition of which is shown in Table 1; add 12% lime milk solution to the acid solution to neutralize excess HCl, then add water to adjust the pH value to 1.5 and the iron ion concentration to 20 g / L to obtain an iron source solution, the composition of which is shown in Table 1;

[0075] Preparation of P salt: Mix wet phosphoric acid with calcium carbonate and calcium oxide for neutralization, and separate impurities to obtain P 2 O 5 / F of the solution is 255, add pure water to adjust the pH value to 2.62, and the P concentration is 33g / L.

[0076] The Fe salt and P salt were synthesized at a ratio of n P / Fe = 1.15, the synthesis temperature was 65°C, the synthesis time was 0.9h, the aging temperature was 93°C, the aging crystallization time was 3h, and the pH of the synthesis mother liquor was 1.6. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0077] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH value to 10 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of pyrite slag.

[0078] Example 3

[0079] Preparation of Fe salt: hydrolyze pyrite slag with hydrochloric acid to obtain an acid solution, the composition of which is shown in Table 1; add 12% lime milk solution to the acid solution to neutralize excess HCl, and then add water to adjust the pH value to 1 and the iron ion concentration to 40 g / L to obtain an iron source solution, the composition of which is shown in Table 1;

[0080] Preparation of P salt: Mix wet phosphoric acid with calcium carbonate and calcium oxide for neutralization, and separate impurities to obtain P 2 O 5 / F of the solution is 260, add pure water to adjust the pH value to 2.65 and the P concentration to 35g / L.

[0081] The Fe salt and the P salt were synthesized at a ratio of n P / Fe = 1.2, the synthesis temperature was 70°C, the synthesis time was 1h, the aging temperature was 94°C, the aging crystallization time was 2h, and the pH of the synthesis mother liquor was 1. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0082] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH value to 12 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of pyrite slag.

[0083] The washed product is dried and calcined to obtain iron phosphate. The obtained iron phosphate product is analyzed, and the results are shown in Figure 2 and Figure 3 , Figure 2 This is a scanning electron microscope photograph of the iron phosphate prepared in Example 3 at a scale of 2 μm. Figure 3 This is a scanning electron microscope photograph of the iron phosphate prepared in Example 3 at a scale of 20 μm. Figure 2 and Figure 3 It can be seen that the product prepared by the method provided by the present invention is spherical particles with good morphology consistency and no obvious agglomeration phenomenon.

[0084] Example 4

[0085] Preparation of Fe salt: hydrolyze pyrite slag with hydrochloric acid to obtain an acid solution, the composition of which is shown in Table 1; add 12% lime milk solution to the acid solution to neutralize excess HCl, and then add water to adjust the pH value to 0.5 and the iron ion concentration to 60 g / L to obtain an iron source solution, the composition of which is shown in Table 1;

[0086] Preparation of P salt: Mix wet phosphoric acid with calcium carbonate and calcium oxide for neutralization, and separate impurities to obtain P 2 O 5 / F of the solution is 280, add pure water to adjust the pH value to 2.7 and the P concentration to 30g / L.

[0087] The Fe salt and P salt were synthesized at a ratio of n P / Fe = 1.6, the synthesis temperature was 65°C, the synthesis time was 1.5 hours, the aging temperature was 99°C, the aging crystallization time was 2 hours, and the pH of the synthesis mother liquor was 0.8. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0088] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH value to 6 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of pyrite slag.

[0089] Example 5

[0090] Preparation of Fe salt: hydrolyze pyrite slag with hydrochloric acid to obtain an acid solution, the composition of which is shown in Table 1; add 12% lime milk solution to the acid solution to neutralize excess HCl, and then add water to adjust the pH value to 0.5 and the iron ion concentration to 80 g / L to obtain an iron source solution, the composition of which is shown in Table 1;

[0091] Preparation of P salt: Mix wet phosphoric acid with calcium carbonate and calcium oxide for neutralization, and separate impurities to obtain P 2 O 5 / F of the solution is 300, add pure water to adjust the pH value to 2.8, and the P concentration is 28g / L.

[0092] The Fe salt and the P salt were synthesized at a ratio of n P / Fe = 1.8, the synthesis temperature was 60°C, the synthesis time was 2h, the aging temperature was 96°C, the aging crystallization time was 2h, and the pH of the synthesis mother liquor was 0.2. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0093] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH value to 7 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of pyrite slag.

[0094] Comparative Example 1

[0095] Preparation of Fe salt: hydrolyze pyrite slag with hydrochloric acid to obtain an acid solution, the composition of which is shown in Table 1; add water to the acid solution to adjust the iron ion concentration to the concentration shown in Table 1, at which the pH value is less than 0 and the iron ion concentration is 40 g / L, to obtain an iron source solution, the composition of which is shown in Table 1;

[0096] Preparation of P salt: Mix wet phosphoric acid with calcium carbonate and calcium oxide for neutralization, and separate impurities to obtain P2 O 5 / F of the solution is 260, add pure water to adjust the pH value to 2.65, the P concentration is 35g / L. .

[0097] The Fe salt and P salt were synthesized at a ratio of n P / Fe = 1.2, the synthesis temperature was 70°C, the aging temperature was 94°C, the aging crystallization time was 4h, and the pH of the synthesis mother liquor was 0.01. After the crystallization was completed, no iron phosphate was produced due to the strong acidity of the slurry.

[0098] Comparative Example 2

[0099] Preparation of Fe salt: hydrolyze pyrite slag with hydrochloric acid to obtain an acid solution, the composition of which is shown in Table 1; add water to the acid solution to adjust the iron ion concentration to that shown in Table 1, at which time the pH value is less than 0 and the iron ion concentration is 40 g / L, to obtain an iron source solution, the composition of which is shown in Table 1;

[0100] Preparation of P salt: Mix wet phosphoric acid with calcium carbonate and calcium oxide for neutralization, and separate impurities to obtain P 2 O 5 / F of the solution is 260, add pure water to adjust the pH value to 2.65 and the P concentration to 35g / L.

[0101] The Fe salt and P salt were synthesized in a ratio of n P / Fe = 1.2, the synthesis temperature was 70°C, 12% ash emulsion solution was added dropwise to adjust the pH value of the slurry; the aging temperature was 94°C, the aging crystallization time was 4h, and the pH value of the synthetic mother liquor was 1. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0102] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH to 10 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of pyrite slag.

[0103] The washed product is dried and calcined to obtain iron phosphate. The obtained iron phosphate product is analyzed, and the results are shown in Figure 4 , Figure 4 This is a scanning electron microscope photo of the iron phosphate prepared in Comparative Example 2. Figure 4 It can be seen that the product prepared by the method provided in Comparative Example 2 has an irregular flaky structure and has obvious agglomeration and poor consistency.

[0104] Example 6

[0105] Preparation of Fe salt: 100g of waste iron mud is hydrolyzed with 432g of 30% hydrochloric acid to separate the acid insoluble matter; air is blown into the acid solution for 30 minutes for oxidation. After the oxidation is completed, 12% ash milk solution is added to the acid solution to neutralize the excess HCl, and pure water is added to prepare an iron source solution with a Fe concentration of 80g / L and a pH value of 0.5.

[0106] Provide P 2 O 5 / F is 300, P concentration is 28g / L, and pH value is 2.8. Monocalcium phosphate solution.

[0107] The Fe salt and the P salt were synthesized at a ratio of n P / Fe = 1.8, the synthesis temperature was 60°C, the synthesis time was 2h, the aging temperature was 96°C, the aging crystallization time was 2h, and the pH of the synthesis mother liquor was 0.2. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0108] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH value to 10 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of waste iron mud.

[0109] Example 7

[0110] Preparation of Fe salt: 100g of waste iron slag was hydrolyzed with 265g of 35% hydrochloric acid to separate the acid insoluble matter; a theoretical amount of 30% H 2 O 2 After oxidation, 12% ash emulsion solution is added dropwise to the acid solution to neutralize excess HCl, and pure water is added to prepare an iron source with an Fe concentration of 40 g / L and a pH value of 1.

[0111] Provide P 2 O 5 / F is 260, P concentration is 35g / L, and pH value is 2.65. Monocalcium phosphate solution.

[0112] The Fe salt and the P salt were synthesized at a ratio of n P / Fe = 1.2, the synthesis temperature was 70°C, the synthesis time was 1h, the aging temperature was 94°C, the aging crystallization time was 2h, and the pH of the synthesis mother liquor was 1. After the crystallization was completed, a separation device was used for solid-liquid separation, and then the product was washed by a combination of online washing and pulping washing.

[0113] The mother liquor obtained by separating the products is neutralized and impurities are removed by adjusting the pH value to 10 with calcium hydroxide, and the slag can be used as white fertilizer. The purified liquid is then supplemented with sulfuric acid to prepare high-quality calcium sulfate and hydrochloric acid, which is circulated to the initial acid hydrolysis stage of waste iron slag.

[0114] The performance of the iron phosphate prepared after washing in the embodiment and the comparative example was tested. The results are shown in Table 2. Table 2 shows the performance test results of the iron phosphate prepared after washing in the embodiment and the comparative example of the present invention.

[0115] Table 2 Performance test results of the iron phosphate prepared after washing in the embodiments of the present invention and the comparative examples

[0116]

[0117] In Table 2, a product is a commercially available product, and its scanning electron microscope photo is as follows: Figure 5 As shown, Figure 5 This is an electron microscope photo of a commercially available iron phosphate product. The product has an irregular flaky structure and obvious agglomeration and poor consistency.

[0118] It can be seen from Table 2 that the total impurity content of the product obtained in the embodiment of the present invention is between 100ppm and 350ppm, and the concentration of a single impurity ion is less than the national limit. The Na ion and K ion of the optimal embodiment are controlled at 20-30ppm, which is much less than the indicators of the products currently sold on the market. Comparative Example 2 is synthesized under the same conditions as Example 3, except that gray milk is not added to the ferric chloride solution to neutralize the excess HCl. Comparative Example 2 is not controlled according to the process of the present invention, and the impurity content of the product obtained is Na ion, K ion, magnesium ion, zinc ion and calcium ion, which are much higher than those in the embodiment of the present invention and do not meet the national standard requirements. In Table 2, a certain product is a commercially available product, and its scanning electron microscope photograph is shown in the figure below. Figure 5 As shown, Figure 5 This is an electron microscope photo of a commercially available iron phosphate product. The product has an irregular flaky structure and obvious agglomeration and poor consistency.

[0119] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing ferric phosphate using iron-containing waste, comprising the following steps: Step a), providing a mixed solution containing ferric chloride obtained by acid hydrolysis of iron-containing waste; The ferric chloride mixed solution is prepared by the following method: using hydrochloric acid to acid-hydrolyze the iron-containing waste material, and then performing oxidation treatment to obtain the ferric chloride mixed solution; Step b), using alkaline compounds and water to adjust the pH value of the ferric chloride mixed solution to meet 0<pH≤2, Fe 3+ The concentration is 10-80 g / L to obtain an iron source solution; Step c), mixing the iron source solution and the monocalcium phosphate solution described in step b) at a molar ratio of P to Fe of 1:1-1.8 to obtain a slurry with a pH value of 0.2-2; the pH value of the monocalcium phosphate solution is 2.5-3.0; Step d), aging and crystallizing the slurry to obtain iron phosphate.

2. The method according to claim 1, characterized in that The ferric chloride mixed solution in step a) comprises: Fe 3 + , Cl - and impurity ions; the impurity ions include Mn 2+ 、Ni 2+ , K + 、Na + Mg 2+ , Cu 2+ 、Zn 2+ and Al 3+ One or more of .

3. The method according to claim 2, characterized in that The mixed solution containing ferric chloride in step a) comprises: 100-200 g / L of Fe 3+ , 200~500 g / L Cl - and impurity ions, wherein the impurity ions include less than 2000 ppm of Mn 2+ 、Ni below 500ppm 2+ , K below 2000ppm + 、Na below 2000ppm + 、Mg below 2000ppm 2+ 、Cu below 500ppm 2+ 、Zn below 500ppm 2+ 、Al below 500ppm 3+ One or more of .

4. The method according to any one of claims 1 to 3, characterized in that: The iron-containing waste is selected from ferrophosphorus, waste iron slag, pyrite cinder, red iron oxide waste or iron-containing chemical sludge.

5. The method according to claim 4, characterized in that In the step b), the alkaline compound is selected from lime milk, lime or limestone.

6. The method according to claim 1, characterized in that In step c), the monocalcium phosphate is prepared from wet-process phosphoric acid and any one or more of lime milk, lime, limestone, calcium phosphate or phosphate rock.

7. The method according to claim 1, characterized in that Step d) also includes solid-liquid separation, mixing the separated mother liquor with an alkaline compound to react to obtain white fertilizer.

8. The method according to claim 7, characterized in that Also includes: The liquid obtained after separating the white fertilizer is mixed with sulfuric acid to react to obtain white gypsum.

9. The method according to claim 8, characterized in that Also includes: The hydrochloric acid obtained after separating the white gypsum is recycled.

10. The method according to claim 1, characterized in that The temperature of the mixed reaction in step c) is 60-70°C and the time is 0.5-2 h; In the step d), the aging and crystallization temperature is 80-99° C. and the time is 2-4 hours.

Citation Information

Patent Citations

  • Method for preparing iron phosphate from calcium dihydrogen phosphate

    CN109928375A

  • Battery-grade ferric phosphate and preparation method

    CN103825024A

  • Urban domestic sludge incineration ash harmless treatment technology and phosphorus compound recycling method

    CN105772484A

  • Preparation method of ferric phosphate

    CN107317029A

  • Method for preparing battery-grade iron phosphate from positive plate of waste lithium iron phosphate battery

    CN109626350A