Low-load bimetallic nanocatalyst, synthesis method and application thereof

Through a low-loading bimetallic catalyst, including Rh and Cs metal atoms, and the carrier is porous carbon, the problem of low reaction activity and many by-products of high-carbon olefins is solved, and the catalytic effect of high activity and stability is achieved, which is suitable for heterogeneous applications. Octene carbonylation reaction.

CN115814833BActive Publication Date: 2024-10-29BEIJING UNIV OF CHEM TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211438542.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-10-29
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

High-carbon olefins have many by-products and low activity in the olefin hydroformylation reaction. Traditional monometallic catalysts have limitations, and the research on disordering of bimetallic catalysts has not been fully developed.

Method used

A low-loading bimetallic catalyst is used, including Rh and Cs metal atoms. The carrier is porous carbon. It is prepared through a specific synthesis method. The mass percentage of Rh is 0.2-0.3% and the mass percentage of Cs is 1.8-2.2%. It is passed through water. The thermal reaction and calcination reduction steps form a highly active catalyst.

Benefits of technology

High metal utilization and low-cost industrial applications are achieved. The catalyst shows excellent activity and stability in the isooctene carbonylation reaction, which is superior to similar catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115814833B_ABST
    Figure CN115814833B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-load bimetallic nanocatalyst, a synthesis method and an application thereof; the low-load bimetallic catalyst comprises an active metal atom Rh and an auxiliary metal Cs, and the carrier is porous carbon; the mass percentage content of the metal atom Rh in the catalyst is 0.2-0.3%; the mass percentage content of the metal atom Cs in the catalyst is 1.8-2.2%. The synthesis method comprises the following steps: 1) preparing a carrier material; 2) preparing an active component impregnation solution; 3) reducing and calcining; 4) adding an auxiliary metal salt; 5) calcining and reducing the bimetallic catalyst. The carbon material-modified bimetallic catalyst prepared by the synthesis method has the activity of different bimetals, wherein the base carbon material is evenly arranged, and the loaded bimetallic Rh-Cs has a relatively high TOF value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalyst synthesis and application, and in particular relates to a low-loaded bimetallic catalyst, a synthesis method and an application thereof, and specifically relates to a low-loaded bimetallic nanocatalyst, a synthesis method and an application thereof. Background Art

[0002] The olefin hydroformylation reaction has been developed for nearly 80 years, during which industrial applications of different types of catalysts have been realized one after another. Among them, the research progress of homogeneous coordination catalysts has been rapidly developed, and the research and development of many types of ligands have become mature. However, with the exploration of scientists, newer technologies have emerged for olefin hydroformylation, from traditional homogeneous catalysts to biphasic catalysts to current solid single-atom catalysts, all of which have been industrially applied. However, the reaction system still remains in the application direction of some short-chain olefins. High-carbon olefins are affected by many by-products and low activity. They have not been developed on a large scale.

[0003] Solid catalysts are reasonable and cheap alternatives to traditional homogeneous catalysts. Single-atom catalytic technology has been recognized by the industry and has begun to develop rapidly. In my country, the industrial application of ethylene relies on single-atom catalysts, but relying solely on a single metal to drive the reaction catalysis often has limitations. Many studies have shown that bimetallic catalysts have an effective effect on improving activity. The development of alloy catalysts has also been reported in many reports. There are geometric and electronic interactions between the parent metal and the co-metal, which can effectively improve the catalytic conversion efficiency and regulate the carbonyl selectivity of olefins. Alloys are ordered bimetallic compounds. The high entropy alloys studied by scientists have also gradually developed recently. Disordered bimetallic catalysts show high activity and stability in carbonylation reactions. Regulating the degree of disorder of bimetallics has become a hot topic in the research field. Summary of the invention

[0004] The first technical problem to be solved by the present invention is to provide a low-loaded bimetallic catalyst.

[0005] The second technical problem to be solved by the present invention is to provide a method for synthesizing a low-load bimetallic catalyst. The carbon material-modified bimetallic catalyst prepared by the synthesis method has the activity of different bimetals, wherein the base carbon material is arranged uniformly, and the loaded bimetallic Rh-Cs has a relatively high TOF value.

[0006] The third technical problem to be solved by the present invention is to provide an application of the bimetallic catalyst obtained by the above synthesis method.

[0007] In order to solve the above-mentioned first technical problem, the present invention adopts the following technical solution:

[0008] A low-loaded bimetallic catalyst comprising:

[0009] Active metal atom Rh and auxiliary metal Cs, the carrier is porous carbon;

[0010] The mass percentage content of the metal atom Rh in the catalyst is 0.2-0.3%;

[0011] The mass percentage content of the metal atom Cs in the catalyst is 1.8-2.2%.

[0012] To solve the above second technical problem, the present invention adopts the following technical solution:

[0013] A method for synthesizing a low-load bimetallic catalyst comprises the following steps:

[0014] 1) Preparation of carrier material

[0015] Weigh 1-3g of carbon source and 5-35g of nitrogen source, add them to 100-300mL of solvent for pre-impregnation, the pre-impregnation time is ≥1h, and then stir evenly to obtain a suspension; hydrothermal reaction for 10-14h, the temperature is greater than the boiling point of distilled water, and the temperature is lowered; then filter, vacuum dry, and then calcine at 500-1000°C to obtain a CN carrier;

[0016] 2) Preparation of active component impregnation solution

[0017] Weigh 0.001-0.01 g of Rh precursor, add it to 20-40 mL of solvent and dissolve it by ultrasonic to obtain an impregnation solution; then 0.05-0.2 g of the carrier is immersed in the impregnation solution and aged for 6-12 hours; the active components are fully diffused, the solid is separated, and it is washed with deionized water for 2-4 times, centrifuged and dried to obtain a Rh single metal catalyst;

[0018] 4) Reduction Calcination

[0019] The Rh monometallic catalyst obtained in step 2) is placed in a tubular furnace, H2 is introduced for calcination reduction, the temperature is programmed to 200-400° C., and the reduction is performed for 3-5 hours to obtain a Rh / CN monometallic catalyst;

[0020] 4) Addition of auxiliary metal salt

[0021] Weigh 0.2-0.4 g of the Rh / CN monometallic catalyst obtained in step 3), add it to 20-40 mL of the auxiliary metal salt solution, and immerse it for 6-10 hours; age it for 6-12 hours, centrifuge and filter the catalyst, and then ultrasonically rinse it with a solvent for 2-3 times, and dry it to obtain a bimetallic catalyst;

[0022] 5) Calcination reduction of bimetallic catalyst

[0023] The bimetallic catalyst obtained in step 4) is placed in a tubular furnace, H2 is introduced for calcination reduction, the temperature is programmed to 500-700°C, and the reduction is performed for 5-7h to obtain the low-load bimetallic catalyst of the product of the present invention.

[0024] As a further improvement of the technical solution, in step 1), the carbon source is porous carbon; and the nitrogen source is an amine compound.

[0025] Preferably, in step 1), the solvent is deionized water.

[0026] As a further improvement of the technical solution, in step 2), the Rh precursor is RhCl3·3H2O.

[0027] Preferably, in step 2), the solvent is deionized water.

[0028] Preferably, in step 2), the immersion temperature is room temperature and the immersion time is 6-10 hours.

[0029] Preferably, in step 2), the cleaning method is ultrasonic cleaning, and the cleaning time is 3-5 minutes.

[0030] As a further improvement of the technical solution, in step 3), the calcination temperature is 200-800°C; more preferably, the calcination temperature is 200-400°C;

[0031] Preferably, in step 4), the auxiliary metal is Cs metal; the auxiliary metal salt is metal nitrate; and the concentration of the auxiliary metal salt solution is 0.002-0.004M.

[0032] Preferably, in step 4), the weight ratio of the metal Rh to the metal Cs is 1:7-9.

[0033] Preferably, in step 5), the calcination temperature is 200-800°C; more preferably, the calcination temperature is 500-700°C.

[0034] In order to solve the third technical problem mentioned above, the present invention also provides an application of a low-loaded bimetallic catalyst obtained by the above synthesis method in olefin carbonylation.

[0035] Any range described in the present invention includes the end value and any numerical value between the end values ​​and any sub-range formed by the end value or any numerical value between the end values.

[0036] Unless otherwise specified, all raw materials in the present invention can be purchased from the market, and the equipment used in the present invention can adopt conventional equipment in the relevant field or refer to the existing technology in the relevant field.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] The bimetallic catalyst with low loading obtained by the present invention has a relatively high metal utilization rate, wherein the CN carrier has loose pores, large specific surface area, and pore diameters concentrated in micropores and mesopores, which is very suitable for the diffusion of metals in the pores; the combination of bimetallics can reflect the interaction and improve the catalytic conversion activity at the same time, and the addition of the auxiliary metal Cs can effectively adjust the electronic morphology of the Rh metal, thereby changing the microenvironment of Rh; at the same time, the precious metal component is reduced to a minimum, thereby achieving low-cost industrial application and ensuring the stability of the apparent activity. This series of catalysts show excellent activity and stability in the catalysis of isooctene carbonylation reaction, which is superior to similar catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The specific embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0040] Figure 1 This is a TEM characterization image of the CsRh bimetallic nanocatalyst obtained in Example 1 of the present invention;

[0041] Figure 2 Schematic diagram of the apparent activity of different bimetallic nanocatalysts obtained in Example 1 of the present invention;

[0042] Figure 3 Schematic diagram of the apparent activity of RhCs bimetallic nanocatalysts with different Rh loadings obtained in Example 1 of the present invention;

[0043] Figure 4 This is the XPS graph of the Cs-Rh bimetallic nanoparticles obtained in Example 1 of the present invention;

[0044] Figure 5 The XRD diagrams of four bimetallic nanocatalysts obtained in Example 1 of the present invention and the comparative example. DETAILED DESCRIPTION

[0045] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0046] As one aspect of the present invention, a low-loaded bimetallic catalyst of the present invention comprises:

[0047] Active metal atom Rh and auxiliary metal Cs, the carrier is porous carbon;

[0048] The mass percentage content of the metal atom Rh in the catalyst is 0.2-0.3%;

[0049] The mass percentage content of the metal atom Cs in the catalyst is 1.8-2.2%.

[0050] As another aspect of the present invention, a method for synthesizing a low-loaded bimetallic catalyst comprises the following steps:

[0051] 1) Preparation of carrier material

[0052] Weigh 1-3g of carbon source and 5-35g of nitrogen source, add them to 100-300mL of solvent for pre-impregnation, the pre-impregnation time is ≥1h, and then stir evenly to obtain a suspension; hydrothermal reaction for 10-15h, the temperature is greater than the boiling point of distilled water, and the temperature is lowered; then filter, vacuum dry, and then calcine at 500-1000°C to obtain a CN carrier;

[0053] 2) Preparation of active component impregnation solution

[0054] Weigh 0.001-0.01 g of Rh precursor, add it to 20-40 mL of solvent and dissolve it by ultrasonic to obtain an impregnation solution; then 0.05-0.2 g of the carrier is immersed in the impregnation solution and aged for 6-12 hours; the active components are fully diffused, the solid is separated, and it is washed with deionized water for 2-4 times, centrifuged and dried to obtain a Rh single metal catalyst;

[0055] 5) Reduction Calcination

[0056] The Rh monometallic catalyst obtained in step 2) is placed in a tubular furnace, H2 is introduced for calcination reduction, the temperature is programmed to 200-400° C., and the reduction is performed for 3-5 hours to obtain a Rh / CN monometallic catalyst;

[0057] 4) Addition of auxiliary metal salt

[0058] Weigh 0.2-0.4 g of the Rh / CN monometallic catalyst obtained in step 3), add it to 20-40 mL of the auxiliary metal salt solution, and immerse it for 6-10 hours; age it for 6-12 hours, centrifuge and filter the catalyst, and then ultrasonically rinse it with a solvent for 2-3 times, and dry it to obtain a bimetallic catalyst;

[0059] 5) Calcination reduction of bimetallic catalyst

[0060] The bimetallic catalyst obtained in step 4) is placed in a tubular furnace, H2 is introduced for calcination reduction, the temperature is programmed to 500-700°C, and the reduction is performed for 5-7h to obtain the low-load bimetallic catalyst of the product of the present invention.

[0061] In certain embodiments of the present invention, in step 1), the carbon source is porous carbon; and the nitrogen source is an amine compound, urea, or a urea homologue.

[0062] In certain embodiments of the present invention, in step 1), the solvent is deionized water.

[0063] In certain embodiments of the present invention, in step 2), the Rh precursor is RhCl3·3H2O.

[0064] In certain embodiments of the present invention, in step 2), the solvent is deionized water.

[0065] In certain embodiments of the present invention, in step 2), the immersion temperature is room temperature and the immersion time is 6-10 hours.

[0066] In certain embodiments of the present invention, in step 2), the cleaning method is ultrasonic cleaning, and the cleaning time is 3-5 minutes.

[0067] In certain embodiments of the present invention, in step 3), the calcination temperature is 200-800°C, or 200-700°C, or 200-600°C, or 200-500°C, or 200-400°C, or 200-300°C, or 300-800°C, or 300-700°C, or 300-600°C, or 300-500°C, or 300-400°C, or 400-800°C, or 400-700°C, or 400-600°C, or 400-500°C, or 500-800°C, or 500-700°C, or 500-600°C, or 600-800°C, or 600-700°C, or 700-800°C; more preferably, the calcination temperature is 200-400°C;

[0068] In certain embodiments of the present invention, in step 4), the auxiliary metal is Cs metal; the auxiliary metal salt is metal nitrate; and the concentration of the auxiliary metal salt solution is 0.002-0.004M.

[0069] In certain embodiments of the present invention, in step 4), the weight ratio of the metal Rh to the metal Cs is 1:7-9.

[0070] In certain embodiments of the present invention, in step 5), the calcination temperature is 200-800°C, or 200-700°C, or 200-600°C, or 200-500°C, or 200-400°C, or 200-300°C, or 300-800°C, or 300-700°C, or 300-600°C, or 300-500°C, or 300-400°C, or 400-800°C, or 400-700°C, or 400-600°C, or 400-500°C, or 500-800°C, or 500-700°C, or 500-600°C, or 600-800°C, or 600-700°C, or 700-800°C; more preferably, the calcination temperature is 500-700°C.

[0071] As another aspect of the present invention, the present invention also provides an application of the bimetallic catalyst obtained by the above synthesis method in olefin carbonylation; preferably, the olefin is isooctene.

[0072] Example 1

[0073] A method for synthesizing a low-load bimetallic catalyst comprises the following steps:

[0074] 1) Preparation of carrier carbon material

[0075] Weigh 1g of carbon source and 10g of nitrogen source. Add 100mL of solvent for pre-impregnation for 2h, then stir evenly to obtain a suspension; transfer to a hydrothermal reactor for hydrothermal reaction for 10h at 120℃, cool down; then filter, vacuum dry, and calcine at 500℃;

[0076] 2) Preparation of active component impregnation solution

[0077] Weigh 0.001 g of Rh precursor, add 20 mL of solvent and ultrasonically dissolve, slowly add 0.05 g of carrier to the impregnation solution, immerse for 6 hours, and age for 6 hours to allow the active components to fully diffuse; separate the solid, wash it twice with deionized water, centrifuge it, and dry it to obtain a Rh single metal catalyst;

[0078] 3) Reduction Calcination

[0079] The Rh monometallic catalyst was placed in a tubular furnace, and H2 was introduced to perform calcination and reduction of the sample. The temperature program was set at 200°C and the reduction was carried out for 4 hours.

[0080] 4) Addition of auxiliary metal salt

[0081] Prepare 20 mL of auxiliary metal salt solution, weigh 0.2 g of Rh / CN single metal catalyst, add it to the auxiliary metal salt solution for immersion; age for 6 hours, centrifuge and filter the catalyst, then ultrasonically rinse it twice with a solvent, and dry it;

[0082] 5) Calcination reduction of samples

[0083] The bimetallic catalyst was placed in a tubular furnace, and H2 was introduced to carry out calcination and reduction operations on the sample. The temperature program was set to 500°C and the reduction was carried out for 5 hours.

[0084] It has been determined that:

[0085] The mass percentage content of the metal atom Rh in the catalyst is 0.25%;

[0086] The mass percentage of the metal atom Cs in the porous carbon in the catalyst is 2%.

[0087] Figure 1 This is a TEM characterization image of the CsRh bimetallic nanocatalyst obtained in Example 1 of the present invention;

[0088] Figure 2 Schematic diagram of the apparent activity of different bimetallic nanocatalysts obtained in Example 1 of the present invention;

[0089] Figure 3 Schematic diagram of the apparent activity of RhCs bimetallic nanocatalysts with different Rh loadings obtained in Example 1 of the present invention;

[0090] Figure 4 This is the XPS graph of the Cs-Rh bimetallic nanoparticles obtained in Example 1 of the present invention;

[0091] Figure 5 The XRD diagrams of four bimetallic nanocatalysts obtained in Example 1 of the present invention and the comparative example.

[0092] Example 2

[0093] A method for synthesizing a low-load bimetallic catalyst comprises the following steps:

[0094] 1) Preparation of carrier carbon material

[0095] Weigh 2g of carbon source and 20g of nitrogen source. Add 200mL of solvent for pre-impregnation for 4h, then stir evenly to obtain a suspension; transfer to a hydrothermal reactor for hydrothermal reaction for 12h at 150℃, cool down; then filter, vacuum dry, and calcine at 700℃;

[0096] 2) Preparation of active component impregnation solution

[0097] Weigh 0.005 g of Rh precursor, add 30 mL of solvent and ultrasonically dissolve, slowly add 0.125 g of carrier to the impregnation solution, immerse for 8 h, and age for 9 h to allow the active components to fully diffuse; separate the solid, wash it with deionized water 3 times, centrifuge it, and dry it to obtain the Rh single metal catalyst;

[0098] 3) Reduction Calcination

[0099] The Rh monometallic catalyst was placed in a tubular furnace, and H2 was introduced to carry out calcination and reduction operations on the sample. The temperature program was set to 300°C and the reduction was carried out for 4 hours.

[0100] 4) Addition of auxiliary metal salt

[0101] Prepare 30 mL of auxiliary metal salt solution, weigh 0.3 g of Rh / CN single metal catalyst, add it into the auxiliary metal salt solution for immersion; age for 9 hours, centrifuge and filter the catalyst, then rinse it with solvent ultrasonically for 3 times, and dry it.

[0102] 5) Calcination reduction of samples

[0103] The bimetallic catalyst was placed in a tubular furnace, and H2 was introduced to carry out calcination and reduction operations on the sample. The temperature program was set to 600°C and the reduction was carried out for 6 hours.

[0104] It has been determined that:

[0105] The mass percentage content of the metal atom Rh in the catalyst is 0.23%;

[0106] The mass percentage of the metal atom Cs in the porous carbon in the catalyst is 1.90%.

[0107] Example 3

[0108] A method for synthesizing a low-load bimetallic catalyst comprises the following steps:

[0109] 1) Preparation of carrier carbon material

[0110] Weigh 3g of carbon source and 35g of nitrogen source. Add 300mL of solvent for pre-impregnation for 6h, then stir evenly to obtain a suspension; transfer to a hydrothermal reactor for hydrothermal reaction for 15h at 180℃, cool down; then filter, vacuum dry, and calcine at 1000℃;

[0111] 2) Preparation of active component impregnation solution

[0112] Weigh 0.01 g of Rh precursor, add 40 mL of solvent and ultrasonically dissolve, slowly add 0.2 g of carrier to the impregnation solution, immerse for 10 h, and age for 12 h to allow the active components to fully diffuse; separate the solid, wash it with deionized water 4 times, centrifuge it, and dry it to obtain the Rh single metal catalyst;

[0113] 3) Reduction Calcination

[0114] The Rh monometallic catalyst was placed in a tubular furnace, and H2 was introduced to carry out calcination and reduction operations on the sample. The temperature program was set to 400°C and the reduction was carried out for 5 hours.

[0115] 4) Addition of auxiliary metal salt

[0116] Prepare 40 mL of auxiliary metal salt solution, weigh 0.4 g of Rh / CN single metal catalyst, add it to the auxiliary metal salt solution for immersion; age for 12 hours, centrifuge and filter the catalyst, then ultrasonically rinse with solvent for 3 times, and dry;

[0117] 5) Calcination reduction of samples

[0118] The bimetallic catalyst was placed in a tubular furnace, and H2 was introduced to carry out calcination and reduction operations on the sample. The temperature program was set to 700°C and the reduction was carried out for 7 hours.

[0119] It has been determined that:

[0120] The mass percentage content of the metal atom Rh in the catalyst is 0.23%;

[0121] The mass percentage of the metal atom Cs in the porous carbon in the catalyst is 1.85%.

[0122] Example 4

[0123] Example 1 was repeated, except that the hydrothermal reaction time in step 1) was adjusted to 15 h.

[0124] Example 5

[0125] Example 1 was repeated, except that the immersion time in step 2) was adjusted to 10 h.

[0126] After testing, both Example 2 and Example 3 can obtain the same technical effect as Example 1. Compared with Example 1, the catalyst of Example 2 maintains the morphology of the carbon substrate, the arrangement remains uniform, and the catalytic activity is not greatly affected; compared with Example 1, the metal particles in Example 3 still maintain a low degree of disordered structure, and the catalytic performance remains good.

[0127] Comparative Example 1

[0128] Example 1 was repeated, except that in step 4), the auxiliary metal salt was a metal salt solution of Fe.

[0129] After testing: the performance of synthesized bimetallic RhFe nanoparticles is inferior to that of CsRh bimetallic catalysts, indicating that different bimetallic nanoparticles have different active centers, see Figure 2 shown.

[0130] Comparative Example 2

[0131] Example 1 was repeated, with the only difference being that in step 4), the auxiliary metal salt was a metal salt solution of Co.

[0132] After testing: Synthesized bimetallic RhCo nanoparticles, their performance is not as good as CsRh bimetallic catalysts, but can form stronger active centers than bimetallic FeRh, see Figure 2 shown.

[0133] Comparative Example 3

[0134] Example 1 was repeated, with the only difference being that in step 4), the auxiliary metal salt was a metal salt solution of Zn.

[0135] After testing: Synthesized bimetallic RhZn nanoparticles, their performance is not as good as CsRh bimetallic catalysts, but can form stronger active centers than bimetallic RhCo, see Figure 2 shown.

[0136] Example 6

[0137] Example 1 was repeated, with the only difference being that in step 2), the amount of Rh added was reduced, and the weight ratio of Cs to Rh was adjusted to 3:2, 2:1, 4:1, and 8:1.

[0138] The results show that the catalytic performance of the obtained catalyst is not significantly decreased compared with that of Example 1, but the Rh content of the precious metal can be reduced to achieve efficient utilization of the metal.

[0139] In summary, the synthesis method of a Co-Rh bimetallic catalyst of the present invention combines multiple investigation angles, reduction calcination temperature, impregnation time, bimetallic types, bimetallic components, etc., which are coordinated and cooperated with each other to form a complete technical solution, so as to obtain the carbon substrate modified bimetallic catalyst required by the present invention.

[0140] Obviously, the above embodiments of the present invention are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

Claims

1. A low-loaded bimetallic catalyst for olefin carbonylation, characterized in that include: Active metal atom Rh and auxiliary metal Cs, the carrier is porous carbon; The mass percentage content of the metal atom Rh in the catalyst is 0.2-0.3%; The mass percentage content of the metal atom Cs in the catalyst is 1.8-2.2%; The method for synthesizing a low-load bimetallic catalyst for olefin carbonylation comprises the following steps: 1) Preparation of carrier material Weigh 1-3g of carbon source and 5-35g of nitrogen source, add them to 100-300mL of solvent for pre-impregnation, the pre-impregnation time is ≥1h, and then stir evenly to obtain a suspension; hydrothermal reaction for 10-14h, the temperature is greater than the boiling point of distilled water, and the temperature is lowered; then filter, vacuum dry, and then calcine at 500-1000°C to obtain a CN carrier; 2) Preparation of active component impregnation solution Weigh 0.001-0.01 g of Rh precursor, add it to 20-40 mL of solvent and dissolve it by ultrasonic to obtain an impregnation solution; Then, 0.05-0.2 g of the carrier is immersed in the impregnation solution and aged for 6-12 hours to allow the active components to fully diffuse, separate the solid, wash it with deionized water 2-4 times, centrifuge it, and dry it to obtain a Rh single metal catalyst; 3) Reduction Calcination The Rh monometallic catalyst obtained in step 2) is placed in a tubular furnace, H2 is introduced for calcination reduction, the temperature is programmed to 200-400° C., and the reduction is performed for 3-5 hours to obtain a Rh / CN monometallic catalyst; 4) Addition of auxiliary metal salt Weigh 0.2-0.4 g of the Rh / CN monometallic catalyst obtained in step 3), add it to 20-40 mL of the auxiliary metal salt solution, and immerse it for 6-10 hours; age it for 6-12 hours, centrifuge and filter the catalyst, and then ultrasonically rinse it with a solvent for 2-3 times, and dry it to obtain a bimetallic catalyst; 5) Calcination reduction of bimetallic catalyst The bimetallic catalyst obtained in step 4) is placed in a tubular furnace, H2 is introduced for calcination reduction, the temperature is programmed to 500-700°C, and the reduction is performed for 5-7h to obtain the product bimetallic catalyst.

2. The bimetallic catalyst according to claim 1, characterized in that: In step 1), the carbon source is porous carbon; and the nitrogen source is an amine compound.

3. The bimetallic catalyst according to claim 1, characterized in that: In step 1), the solvent is deionized water.

4. The bimetallic catalyst according to claim 1, characterized in that: In step 2), the Rh precursor is RhCl3·3H2O.

5. The bimetallic catalyst according to claim 1, characterized in that: In step 2), the solvent is deionized water.

6. The bimetallic catalyst according to claim 1, characterized in that: In step 2), the immersion temperature is room temperature and the immersion time is 6-10 hours.

7. The bimetallic catalyst according to claim 1, characterized in that: In step 2), the cleaning method is ultrasonic cleaning, and the cleaning time is 3-5 minutes.

8. The bimetallic catalyst according to claim 1, characterized in that: In step 4), the auxiliary metal is Cs metal; the auxiliary metal salt is metal nitrate; and the concentration of the auxiliary metal salt solution is 0.002-0.004M.

9. The bimetallic catalyst according to claim 1, characterized in that: In step 4), the weight ratio of the metal Rh to the metal Cs is 1:7-9.

Citation Information

Patent Citations

  • Bisphosphite compounds, the metal complexes thereof and the use of said compounds and complexes in olefin hydroformylation

    AU2001278460A1

  • Application of supported catalyst in olefin hydroformylation reaction

    CN112973678A

  • Method for preparing cyclohexanecarboxylic acid through fixed bed catalytic benzoic acid hydrogenation

    CN114433164A

  • Preparation method and application of N-doped porous carbon material loaded bimetallic catalyst

    CN114602497A

  • Multiphase Rh-Li metal catalyst for methanol carbonylation and its prepn

    CN1349852A