An efficient acoustic resonance mixing method for composite high-energy ball milling
By adding spherical dielectric materials and vacuum technology to the acoustic resonance mixing, the agglomerated ultrafine powder materials are broken and disassembled, and the problem of poor mixing uniformity of ultrafine powder materials in the prior art is solved, and efficient superhard material mixing and Performance improvement.
Patent Information
- Application Number
- CN202211647887.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-21
AI Technical Summary
The existing acoustic resonance mixing technology is difficult to achieve uniform mixing of ultrafine powder materials, and traditional methods are difficult to crush and disaggregate ultrafine powder materials, resulting in poor mixing uniformity and limiting the performance improvement of superhard materials.
Using the highly efficient acoustic resonance mixing method of composite high-energy ball mill, the uniform dispersion of the ultrafine powder material is achieved by adding 0.1~10mm spherical dielectric material to the raw materials, and the violent vibration crushing and vacuum deaggregation during mixing.
It realizes efficient and uniform mixing of ultrafine powder materials, improves product performance, ensures high mixing uniformity of superhard materials and consistent performance of batch production, and has a higher mixing efficiency than traditional three-dimensional mixing machines.
Smart Images

Figure CN115815607B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of material technology, including but not limited to superhard materials, powder metallurgy, chemical industry, medicine and other fields, and particularly relates to a high-efficiency acoustic resonance mixing method of composite high-energy ball milling. Background Art
[0002] Resonant Acoustic Mixing (RAM) is a new technology that has emerged in recent years based on the coupling of macroscopic vibration mixing and microscopic mixing of acoustic fields. It uses the resonance of a mechanical vibration system to generate high-intensity vibration excitation, which excites low-frequency, high-acceleration sound waves in multiphase flow, and achieves uniform mixing of materials under the excitation of sound waves. RAM forms uniform microscale mixing units in the entire mixing field, without dead corners, and can achieve solid-solid, solid-liquid, and liquid-liquid mixing. RAM technology is a new mixing technology funded and developed by the U.S. Department of Defense. It was first used in the field of ammunition manufacturing and was praised by foreign technical experts as a "game-changing disruptive technology" in the field of mixing energetic materials and other materials. RAM technology has the advantages of high mixing efficiency, good uniformity, and low dangerous stimulation. It is also gradually being used in medicine, materials, batteries, biology and other fields besides military industry.
[0003] The domestic units engaged in the development of acoustic resonance hybrid technology mainly include Zhengzhou Grinding Tool and Abrasive Grinding Research Institute Co., Ltd. At present, domestic acoustic resonance hybrid technology is mainly used in the military field, and experimental verification has also begun in the fields of superhard materials, fine cosmetics, pharmaceuticals, batteries, etc. Acoustic resonance hybrid technology has great application potential in the superhard materials industry. With the development of the industry, the improvement of precision / ultra-precision machining technology, the particle size of the raw materials of the corresponding superhard material tools is also getting finer and finer. The internationally advanced PDC (polycrystalline diamond composite) products have begun to use 1μm diamond powder, and even nano-level PDC has been successfully synthesized. In addition to PDC products, the raw materials (diamond powder, binder powder, etc.) used in other superhard material products for precision machining (super-fine oilstone, wafer thinning grinding wheel, etc.) are also gradually refined to below 5μm. As the particle size of raw materials becomes finer, the surface energy of the raw materials increases and they are very easy to agglomerate. The uniformity of raw material mixing has become a bottleneck restricting the development of high-performance superhard material products. Using traditional three-dimensional mixers, it is difficult to achieve uniform mixing of ultrafine powder materials by extending the mixing time and changing the mixing conditions.
[0004] Among the existing acoustic resonance mixing technologies, most of them are aimed at the application of acoustic resonance mixing technology on energetic materials. At the same time, for 40μm and coarser materials that are not easy to agglomerate, acoustic resonance mixing can give full play to the advantages of high-energy vibration technology and quickly achieve uniform dispersion, but there is currently a lack of effective technology for achieving uniform mixing of ultrafine powder materials. CN108043305A discloses a method for preparing a solid propellant paddle without a paddle. In the first step of the method, the material to be mixed is heated to a certain temperature (25~125℃), and then the acoustic resonance mixer is started for mixing. In the second step, the mixing container is evacuated (1kPa~20kPa), and then acoustic resonance mixing is performed. When acoustic resonance mixing is used, the mixing acceleration is 0~110g and the mixing time is 5~25min. This patent assists the acoustic resonance mixing process by heating and vacuum, and can obtain a solid propellant paddle by a paddle-free mixing method, but it cannot solve the problem of agglomeration of ultrafine powder materials. The reason is that most of the existing acoustic resonance mixing technology solutions only change the basic equipment function parameters such as acoustic resonance mixing acceleration and mixing time. Although the technical advantages of acoustic resonance mixing, such as violent vibration and large amplitude, are utilized to allow the materials to fully exchange positions and move, it is difficult to effectively break up and de-agglomerate the agglomerated materials. Even if the process parameters such as the mixing time are greatly extended, the effect is minimal, and the agglomerates still exist in the end, resulting in single acoustic resonance mixing being difficult to effectively achieve uniform dispersion of ultrafine powder materials. Summary of the invention
[0005] The purpose of the present invention is to provide an efficient acoustic resonance mixing method of composite high-energy ball milling in view of the deficiencies of the above-mentioned prior art, so as to achieve uniform distribution of ultrafine raw materials, meet the requirements of uniform mixing of products, and further improve product performance.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] A high-efficiency acoustic resonance mixing method for composite high-energy ball milling comprises the following steps:
[0008] (1) Select ultra-fine raw material powder;
[0009] (2) According to the quality of raw materials required for the product, select a mixing tank of appropriate size, and the volume ratio of the raw materials filling the mixing tank should be 20%~80%;
[0010] (3) After adding the raw material powder into the mixing tank, add an appropriate amount of spherical medium material, and select the appropriate ball milling medium according to the composition and particle size of the mixed raw materials. The size of the spherical medium material is 0.1~10mm, and the filling ratio is based on the material of the spherical medium. The medium / raw material mass ratio is 1:1~10:1, or the medium / raw material volume ratio is 1:1~3:1;
[0011] (4) Evacuate the mixing tank to a vacuum degree of 1-1000 Pa, and heat it at a temperature of 25-150°C depending on the raw materials;
[0012] (5) Place the pre-evacuated or pre-heated mixing tank on an acoustic resonance mixer for a mixing test;
[0013] (6) The mixed material obtained in step (5) is screened and then subjected to subsequent production and processing to obtain a superhard material product.
[0014] In step (1), the raw material powder includes, but is not limited to, ultra-fine oilstone powder material composed of ultra-fine diamond powder and binder powder of less than 10 μm, wafer thinning grinding wheel powder material, and resin bond grinding wheel powder material.
[0015] In step (3), the spherical dielectric material includes but is not limited to PC, PP, acrylic, POM, cemented carbide, stainless steel, zirconia, alumina, etc.
[0016] In step (3), the material of the mixing tank includes but is not limited to PP, PC, and stainless steel.
[0017] In step (5), the mixing process is: mixing acceleration 30-100 g, mixing time 5-30 min.
[0018] The beneficial effects of the present invention are:
[0019] (1) The present invention discloses a high-efficiency acoustic resonance mixing method for composite high-energy ball milling. By adding 0.1-10 mm spherical medium materials into raw materials, the spherical medium vibrates violently together with the powder during mixing, and collides with the agglomerated powder during the movement, so that the agglomerated powder can be effectively crushed, deagglomerated, and refined to achieve effective dispersion. At the same time, vacuuming is performed before mixing to assist in deagglomeration of the agglomerated powder, and finally a uniformly mixed raw material is obtained, which can meet the requirements of ultra-high performance superhard material products for high mixing uniformity of raw materials. Ultrafine powder materials mixed by this method, such as ultra-fine oilstone powder materials, wafer thinning grinding wheel powder materials, etc., can achieve uniform distribution of ultrafine raw materials, meet the requirements of uniform mixing of products, and further improve product performance.
[0020] (2) The acoustic resonance mixing technology of the composite high-energy ball mill can quickly and effectively achieve uniform mixing of ultrafine powders, uniform dispersion of abrasives and binders, and uniform loss of diamonds and binders during grinding of sintered products, which has beneficial effects on the hardness, wear, and grinding consistency of the product.
[0021] (3) This mixing technology uses independent tanks for mixing, with raw materials, spherical media, and mixing tanks corresponding one to one, avoiding trace element contamination when mixing different materials and ensuring the consistency and stability of product performance during mass production.
[0022] (4) This mixing technology can achieve uniform mixing of ultrafine powder materials within 5 to 25 minutes, and the mixing efficiency is up to 10 times that of traditional three-dimensional mixers. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a production flow chart of the present invention;
[0024] Figure 2 It is a schematic diagram of the mixing effect of the existing traditional three-dimensional mixer;
[0025] Figure 3 It is a schematic diagram of the existing composite high-energy ball mill acoustic resonance mixing effect;
[0026] Figure 4 It is a schematic diagram of the existing composite high-energy ball mill acoustic resonance mixed deagglomeration, crushing and refinement;
[0027] Figure 5 This is a comparison diagram of the two mixing effects of the super refined oil stone in Example 1;
[0028] Figure 6 This is a comparison diagram of two mixed effects of wafer thinning grinding wheels in Example 2;
[0029] Figure 7 This is a comparison chart of the two mixing effects of the resin bond grinding wheel in Example 3. DETAILED DESCRIPTION
[0030] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0031] The present invention provides a highly efficient acoustic resonance mixing method for composite high energy ball milling, such as Figures 1 to 7 shown.
[0032] A highly efficient acoustic resonance mixing technology for composite high-energy ball milling, the mixing steps are as follows:
[0033] (1) The ultrafine powder material in the present invention includes, but is not limited to, ultrafine oilstone powder material composed of ultrafine diamond powder of less than 10 μm and binder powder, wafer thinning grinding wheel powder material, resin bond grinding wheel powder material, etc.
[0034] (2) Select a mixing tank of appropriate size based on the quality of raw materials required for specific products. Ensure that the volume ratio of raw materials filling the mixing tank is 20%~80%. The materials of the mixing tank include but are not limited to PP, PC, stainless steel, etc.
[0035] (3) After adding the raw material powder into the mixing tank, add an appropriate amount of spherical medium material. Select appropriate ball milling media according to the composition and particle size of the raw materials to be mixed. Spherical medium materials include but are not limited to PC, PP, acrylic, POM, cemented carbide, stainless steel, zirconium oxide, aluminum oxide, etc. The size of the spherical medium material is 0.1~10mm, and the filling ratio can be selected according to the material of the spherical medium. The medium / raw material mass ratio can be 1:1~10:1, or the medium / raw material volume ratio can be 1:1~3:1.
[0036] (4) Evacuate the mixing tank to a vacuum degree of 1-1000 Pa. The raw materials can be heated according to their specific requirements at a temperature of 25-150°C.
[0037] (5) Place the pre-vacuumed or pre-heated mixing tank on an acoustic resonance mixer for a mixing test. The mixing process is: mixing acceleration 30-100g, mixing time 5-30min.
[0038] (6) The mixed material obtained in step 5 is screened and then subjected to subsequent production and processing to obtain a superhard material product.
[0039] The present invention will be further described below in conjunction with specific embodiments:
[0040] Example 1
[0041] A highly efficient acoustic resonance mixing technology of composite high-energy ball milling. The mixed raw materials are ultra-fine oil stone raw materials with a particle size of 5 μm or finer. The specific mixing steps are as follows:
[0042] (1) The raw materials of super refined oilstone are composed of 5μm fine diamond powder and ceramic binder powder.
[0043] (2) According to the product formula, weigh 200g of raw material powder and select a 500ml PC mixing tank.
[0044] (3) Add the raw material powder into the mixing tank, select PP spherical medium with a particle size of 6 mm, and add it into the mixing tank. The volume ratio of spherical medium to raw material is 1.5:1.
[0045] (4) Evacuate the mixing tank to a vacuum degree below 10 Pa.
[0046] (5) Place the mixing tank on an acoustic resonance mixer for a mixing test with a mixing acceleration of 50 g and a mixing time of 15 min.
[0047] (6) Take out the material in the mixing tank, sieve out the spherical medium, and obtain a uniformly mixed powder material. The powder material is processed according to the process flow to obtain a super refined oil stone product.
[0048] The uniformly mixed powder material obtained in Example 1 was subjected to SEM testing and compared with the powder material obtained by using a traditional three-dimensional mixer at the same mixing time. Figure 1 As shown. After 15 minutes of mixing with the traditional three-dimensional mixer, binder agglomeration still exists in the powder material. Under the same conditions, the powder of the composite high-energy ball mill acoustic resonance mixing technology is evenly dispersed without obvious agglomeration. The organizational uniformity and performance stability of the sintered product are better than those of the sintered products of the traditional mixing equipment.
[0049] Example 2
[0050] A highly efficient acoustic resonance mixing technology for composite high-energy ball milling. The mixed raw materials are wafer thinning grinding wheel raw materials, and the diamond abrasive particle size is 1μm. The specific mixing steps are as follows:
[0051] (1) The wafer thinning grinding wheel is composed of diamond micropowder with an average particle size of 1 μm and ceramic binder micropowder.
[0052] (2) Weigh 100 g of raw material powder according to the product formula and select a 100 ml PC mixing tank.
[0053] (3) Add the raw material powder into the mixing tank, select alumina spherical media with a particle size of 4 mm, and add it into the mixing tank. The mass ratio of spherical media to raw material is 3:1.
[0054] (4) Evacuate the mixing tank to a vacuum degree below 10 Pa.
[0055] (5) Place the mixing tank on an acoustic resonance mixer for a mixing test with a mixing acceleration of 60 g and a mixing time of 20 min.
[0056] (6) Take out the material in the mixing tank, sieve out the spherical medium, and obtain a uniformly mixed powder material. The powder material is subsequently processed according to the process flow to obtain a wafer thinning grinding wheel product.
[0057] The uniformly mixed powder material obtained in Example 2 was subjected to SEM testing and compared with the powder material obtained by using a traditional three-dimensional mixer at the same mixing time. Figure 2 As shown. After 20 minutes of mixing with the traditional three-dimensional mixer, there are still a lot of binder agglomerates in the powder material. Under the same conditions, the composite high-energy ball milling acoustic resonance mixing technology disperses the powder evenly without obvious binder agglomeration. The sintered product has high hardness, low wear and long grinding life.
[0058] Example 3
[0059] A high-efficiency acoustic resonance mixing technology for composite high-energy ball milling. The mixed raw materials are resin bond grinding wheel raw materials, and the resin bond particle size is 1 μm. The specific mixing steps are as follows:
[0060] (1) The resin bond grinding wheel is composed of diamond powder with an average particle size of 1 μm and resin bond powder.
[0061] (2) According to the product formula, weigh 150g of raw material powder and select a 500ml PC mixing tank.
[0062] (3) Add the raw material powder into the mixing tank, select alumina spherical media with a particle size of 3 mm, and add it into the mixing tank. The mass ratio of spherical media to raw material is 5:1.
[0063] (4) Evacuate the mixing tank to a vacuum degree below 10 Pa.
[0064] (5) Place the mixing tank on an acoustic resonance mixer for a mixing test with a mixing acceleration of 70 g and a mixing time of 25 min.
[0065] (6) Take out the material from the mixing tank, sieve out the spherical medium, and obtain a uniformly mixed powder material. The powder material is subsequently processed according to the process flow to obtain a resin bonded grinding wheel product.
[0066] The uniformly mixed powder material obtained in Example 3 was subjected to SEM testing and compared with the powder material obtained by using a traditional three-dimensional mixer at the same mixing time. Figure 3 As shown. After 25 minutes of mixing with a traditional three-dimensional mixer, a large amount of binder agglomerates still exist in the powder material. Under the same conditions, the composite high-energy ball milling acoustic resonance mixing technology disperses the powder evenly without obvious binder agglomeration. The sintered product has a low load on the workpiece being ground, small load fluctuation, and a long service life.
[0067] Acoustic resonance mixing technology achieves uniform mixing of mixed materials through the coupling of macroscopic vibration mixing and microscopic acoustic flow mixing, but the mixing effect for ultrafine powder materials (raw material particle size ≤ 10μm) is general. The main reason is that ultrafine powders are very easy to agglomerate into large particles. It is difficult to effectively break and de-agglomerate the agglomerated materials when mixed under traditional processes. Even if the mixing time and other process parameters are greatly extended, the effect is minimal. Agglomeration still exists in the end, resulting in single acoustic resonance mixing. It is difficult to effectively achieve uniform dispersion of ultrafine powder materials. The present invention adds 1~10mm spherical medium materials (the size, material and quality of the spherical medium are selected according to the physicochemical properties of the raw materials to be mixed) to the raw materials. During mixing, the spherical medium vibrates violently with the powder, collides with the agglomerated powder during the movement, and can achieve effective crushing, de-agglomeration, refinement and effective dispersion of the agglomerated powder. At the same time, vacuuming before mixing can assist in the de-agglomeration of the agglomerated powder. Finally, the raw materials are mixed evenly, which can meet the requirements of ultra-high performance superhard material products for high mixing uniformity of raw materials.
[0068] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the invention claimed for protection. The scope of protection claimed for the present invention is defined by the attached claims and their equivalents.
[0069] In the description of the present invention, it is necessary to understand that the terms "front", "rear", "left", "right", "center", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the protection content of the present invention.
Claims
1. A high-efficiency acoustic resonance mixing method for composite high-energy ball milling, characterized in that: The following steps are involved: (1) Select ultra-fine raw material powder; Raw material powders include, but are not limited to, ultra-fine oilstone powder materials composed of ultra-fine diamond powder and binder powder of less than 10 μm, wafer thinning grinding wheel powder materials, and resin bond grinding wheel powder materials; (2) According to the quality of raw materials required by the product, select a mixing tank of appropriate size, and the volume ratio of the raw materials filling the mixing tank should be 20%~80%; (3) After adding the raw material powder into the mixing tank, add an appropriate amount of spherical medium material, and select the appropriate ball milling medium according to the composition and particle size of the mixed raw materials. The size of the spherical medium material is 0.1~10mm, and the filling ratio is based on the material of the spherical medium. The medium / raw material mass ratio is 1:1~10:1, or the medium / raw material volume ratio is 1:1~3:1; (4) Evacuate the mixing tank to a vacuum degree of 1-1000 Pa, and heat it at a temperature of 25-150°C depending on the raw materials; (5) Place the pre-vacuumed or pre-heated mixing tank on an acoustic resonance mixer for a mixing test. The mixing process is: mixing acceleration 30-100g, mixing time 5-30min; (6) The mixed material obtained in step (5) is screened and then subjected to subsequent production and processing to obtain a superhard material product.
2. The high-efficiency acoustic resonance mixing method of composite high-energy ball milling according to claim 1, characterized in that: In step (3), the spherical medium material includes but is not limited to PC, PP, acrylic, POM, cemented carbide, stainless steel, zirconium oxide, and aluminum oxide.
3. The high-efficiency acoustic resonance mixing method of composite high-energy ball milling according to claim 1, characterized in that: In step (3), the material of the mixing tank includes but is not limited to PP, PC, and stainless steel.