A method for extracting lithium from salt lake brine and controlling the impurity content of desorption solution
Through multi-stage countercurrent washing and acid supplementation technology, the problem of insufficient selectivity of impurity elements in the lithium extraction process of salt lake brine is solved, the impurity content of the absorbed liquid is reduced, the lithium recovery rate and product quality are improved, and the power consumption and fresh water are reduced. Use amount.
Patent Information
- Application Number
- CN202211470970.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-23
AI Technical Summary
In the existing salt lake brine lithium extraction process, the adsorbent is insufficient to selectively impurities, resulting in high content of impurities such as sodium and potassium in the desorption solution, affecting subsequent impurity removal and concentration processes, increasing power consumption and reducing lithium recovery and product quality. .
By adding acid to the washing liquid, the sodium, potassium, magnesium and other elements co-adsorbed in the adsorbent are effectively elutioned, and the impurity content of the desorbent is reduced, and the elution of the impurity elements of the desorbent is combined with rinsing and co-adsorbed impurity elements. , adjust the acid supplement to reduce impurities entering the desorption solution.
It significantly reduces the impurity content in the adsorption liquid, reduces the burden of subsequent impurity removal, reduces the power consumption of electrodialysis, and improves the recovery rate and product quality of MVR and multi-effect evaporated crystalline lithium hydroxide.
Smart Images

Figure CN115818673B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium extraction from salt lake brine, and in particular to a method for controlling the impurity content of a desorption liquid during lithium extraction from salt lake brine. Background Art
[0002] With the development of new energy industry, the lithium battery industry has developed by leaps and bounds, and with it comes the exponential growth of demand for lithium resources. More than 70% of the world's lithium resources exist in salt lake lithium mines. At present, the main processes for extracting lithium from salt lakes include salt drying process, adsorption process, membrane process, electrochemical deintercalation process, etc. my country's salt lake resources are mainly distributed in Qinghai, Tibet, Xinjiang and Hubei, among which Qinghai and Tibet account for 74% of the country's lithium resource reserves. Most of the Qinghai salt lakes are high magnesium-lithium ratio salt lakes, and the brine is weakly acidic or neutral. Due to different geology, most of the Tibetan salt lakes are alkaline brines, and the typical one is the Zabuye carbonate salt lake.
[0003] The adsorbents used in the adsorption process mainly include aluminum, titanium and manganese adsorbents. Aluminum adsorbents are molecular sieves with good lithium-sodium and lithium-magnesium separation characteristics and chemical stability in neutral brine. They have been industrialized in Qinghai, but they are only suitable for chloride-type salt lakes, have low adsorption capacity, large fresh water consumption, and cannot effectively enrich lithium. Manganese adsorbents are ion sieves with large adsorption capacity, but poor chemical stability and large dissolution loss. Titanium adsorbents are also ion sieves, and their stability and dissolution rate are better than manganese adsorbents. They can be used in sodium sulfate subtype or carbonate salt lakes, and lithium can be effectively enriched after acid desorption. Chinese patent application CN110106356A provides a method for extracting lithium using a powdered titanium ion exchanger. The brine is stirred in an ion exchange tank for adsorption and extraction of lithium. After filtration and desorption, a lithium-rich solution is obtained. The lithium concentration in the solution can reach more than 10g / L, and the sodium concentration is 1.6-1.7g / L. However, the powdered adsorption material has high dissolution loss and is difficult to filter, so it is not industrially feasible.
[0004] For complex salt lake brine systems, some impurity elements will be chemically adsorbed by the adsorbent, and when the adsorption capacity is low, the Na / Li in the desorption solution will increase. High content of impurities such as sodium and potassium in the desorption solution will have a great impact on the back-end impurity removal and concentration process, significantly increase the energy consumption of electrodialysis, and greatly reduce the yield and product quality of MVR evaporation crystallization of lithium hydroxide monohydrate.
[0005] Chinese patent application CN112777614A discloses a method for reducing Na / Li in desorption solution by pre-desorption. The invention sets a pre-desorption step for the loaded granulated titanium adsorbent after washing with clean water, and uses a weak acid solution for pre-desorption. This method has some obvious defects. First, the lithium content in the pre-desorption liquid is high, and the return to the adsorption process causes the loss of part of the capacity of the adsorbent; second, the adsorbent after pre-desorption has no clean water washing operation, and the impurities in the pre-desorption liquid remaining in the column will enter the desorption liquid, weakening the separation effect of the pre-desorption impurities; third, the independent washing and pre-desorption processes will extend the lithium extraction cycle and further reduce the equipment capacity. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention aims to provide a method for extracting lithium from salt lake brine and controlling the impurity content of the desorption solution.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A method for extracting lithium from salt lake brine to control the impurity content of the desorption liquid, utilizing the difference in the adsorption characteristics of the adsorbent for lithium and sodium, and strengthening the adsorption conditions to increase the lithium adsorption capacity of the adsorbent. The co-adsorbed elements such as sodium, potassium, and magnesium are eluted by multi-stage countercurrent washing of the loaded adsorption column and adding acid to the washing liquid, which can effectively reduce the impurity content in the desorption liquid. The specific process is:
[0009] S1. Use a continuous ion exchange device to adsorb lithium in lithium-containing salt lake brine passing through an adsorption column after loading a lithium-extracting adsorbent. The tail brine after adsorption flows out of the continuous ion exchange device and returns to the salt lake. The loaded adsorption column carrying brine enters the last stage of a multi-stage countercurrent washing system for washing.
[0010] S2, clean water or a solution of clean water with diluted acid added enters the first-stage washing column, and the load adsorption column is subjected to multi-stage countercurrent washing, and the co-adsorbed sodium, potassium and magnesium elements are eluted while washing the load adsorption column; the washing liquid flowing out of each washing column is supplemented with diluted acid to adjust the acid concentration and then enters the next-stage washing column, and the washing liquid flowing out of the last-stage washing column is returned to the salt lake through a pipeline;
[0011] S3. The washed adsorption column is moved to a desorption zone for desorption to obtain a lithium-rich desorption solution, and the lithium-rich desorption solution is concentrated and impurities are removed to prepare lithium hydroxide monohydrate or lithium carbonate products.
[0012] Furthermore, in step S1, when lithium in lithium-containing salt lake brine passing through the adsorption column is adsorbed, the lithium adsorption capacity of the adsorbent is increased to 4-21 mg / g by increasing the amount of brine input.
[0013] Furthermore, in step S1, the lithium extraction adsorbent is a titanium adsorbent, such as lithium metatitanate Li2TiO3 and lithium titanate Li4Ti5O 12 One or a mixture of two.
[0014] Furthermore, in step S1, the lithium-containing salt lake brine is an alkaline brine with a pH value greater than 7, a lithium content of 100 mg / L-2000 mg / L, a sodium content of 1-150 g / L, a potassium content of 0.1 g / L-35 g / L, and a magnesium content of 0.1 g / L-10 g / L; the alkaline brine includes one or more of alkaline sodium sulfate subtype salt lake brine, carbonate brine and lithium precipitation mother liquor.
[0015] Furthermore, in step S2, the clean water includes one or more of surface river water, groundwater, softened water, membrane-treated desalted water, and pure water.
[0016] Furthermore, in step S2, the dilute acid is dilute hydrochloric acid or dilute sulfuric acid.
[0017] Furthermore, in step S2, the dilute acid added to the clean water and each level of washing liquid is concentrated hydrochloric acid or an aqueous solution prepared by adding concentrated hydrochloric acid to water, or a dilute sulfuric acid or dilute hydrochloric acid solution produced by a bipolar membrane electrodialysis process.
[0018] Further, in step S2, after adding the dilute acid, the H + The arithmetic sum of the concentrations is 0.02-0.1 mol / L, distributed according to the order.
[0019] Furthermore, in step S2, the method of adding dilute acid is as follows: the washing liquid flowing out of each stage enters a separate buffer tank, and dilute acid is added to adjust the acid concentration before entering the next washing column; or a dilute acid adding pipe is connected to the washing liquid delivery pipeline to add dilute acid online, and the washing liquid pH at the washing column inlet is measured by an online pH meter and a flow meter. + The concentration can be controlled by adding the washing liquid and the dilute acid from the top of the adsorption column at the same time, and the H in the washing liquid after mixing can be controlled by the flow rate of the washing liquid and the dilute acid. + concentration.
[0020] Furthermore, in step S2, the number of series-connected stages of the multi-stage countercurrent washing is 2-6 stages.
[0021] Further, in step S2, when the number of series-connected multi-stage countercurrent washing stages is 4, the clean water or the solution H after adding dilute acid to the clean water entering the first-stage washing column + The concentration is 0-0.02mol / L. When the washing liquid from the first-stage washing column flows into the second-stage washing column after adding dilute acid, H +The concentration is 0.01-0.06mol / L. When the washing liquid flowing out of the second-stage washing column flows into the third-stage washing column after adding dilute acid, H + The concentration is 0.01-0.06mol / L. When the washing liquid flowing out of the third-stage washing column flows into the fourth-stage washing column after adding dilute acid, H + The concentration is 0-0.05mol / L.
[0022] Furthermore, in step S2, the washing flow rate is 1-10 BV / h.
[0023] Furthermore, in step S2, the amount of clean water used during washing is 0.6-5 BV, which is determined according to the impurity content of the brine, the number of washing stages in series and the water balance requirement.
[0024] Furthermore, in step S2, during the multi-stage countercurrent washing process, the temperature of the solution and each stage of washing liquid is 1°C-50°C.
[0025] Furthermore, in step S2, the washing liquid of each washing column flows in a direction of top-in and bottom-out or bottom-in and top-out, or the two flow directions are arranged and combined between different washing columns.
[0026] The beneficial effects of the present invention are:
[0027] (1) In the lithium extraction technology of salt lake by adsorption, the concentration of impurity elements in the desorption liquid of titanium adsorbent is high due to the selectivity of titanium adsorbent for elements such as sodium, potassium, and magnesium. In particular, excessive sodium and potassium are difficult to separate from lithium. In the multi-stage countercurrent washing stage of the continuous separation device loaded with adsorbent, the present invention can effectively remove the sodium, potassium, magnesium and other elements co-adsorbed in the adsorbent while washing away the tail halides in the loaded adsorbent, thereby greatly reducing the impurity content of the desorption liquid by adding acid to the washing liquid.
[0028] (2) The present invention realizes the combination of elution and elution of co-adsorbed impurity elements, and can flexibly adjust the amount of acid added in each stage of the washing column. By adjusting the amount of acid added at different stages, the amount of impurities entrained into the desorption liquid with the washing liquid can be reduced.
[0029] (3) The present invention can elute the co-adsorbed impurity elements, especially sodium and potassium, while washing the loaded adsorbent, which can effectively reduce the burden of subsequent impurity removal and the power consumption of qualified liquid during electrodialysis concentration, and can also greatly improve the lithium recovery rate and product quality during MVR and multi-effect evaporation crystallization of lithium hydroxide monohydrate.
[0030] (4) The present invention combines the elution of co-adsorbed impurity elements with the washing of entrained brine, which can effectively reduce the use of fresh water. This is particularly important for lithium-containing salt lakes, which are mostly located in inland areas with dry climates and shortage of fresh water resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of a method flow of an embodiment of the present invention;
[0032] Figure 2 A schematic diagram of device connections for implementing the method according to an embodiment of the present invention.
[0033] Explanation of reference numerals: 1-18, adsorption column; 19-26, desorption washing column; 27, first-stage washing column; 28, second-stage washing column; 29, third-stage washing column; 30, fourth-stage washing column; 31, adsorption zone; 32, desorption zone; 33, dilute acid storage tank; 34, clean water storage tank; 35, first-stage washing liquid buffer tank; 36, second-stage washing liquid buffer tank; 37, third-stage washing liquid buffer tank; 38, adsorption tail brine tank. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0035] This embodiment provides a method for extracting lithium from salt lake brine and controlling the impurity content of the desorption liquid. The difference in the adsorption characteristics of the adsorbent for lithium and sodium is utilized to enhance the adsorption conditions to improve the lithium adsorption capacity of the adsorbent. By washing the loaded adsorption column with multi-stage countercurrent and adding acid in the washing liquid in stages, the co-adsorbed elements such as sodium, potassium, and magnesium are eluted while washing the loaded adsorption column, which can effectively reduce the impurity content in the desorption liquid.
[0036] like Figure 1 As shown, the specific process of the above method is:
[0037] S1. After loading the lithium-extracting adsorbent, the lithium in the lithium-containing salt lake brine passing through the adsorption columns 1-18 in the adsorption zone 31 is adsorbed using a continuous ion exchange device. The tail brine after adsorption flows out of the continuous ion exchange device and returns to the salt lake. The loaded adsorption column containing the entrained brine enters the last washing column 30 of the multi-stage countercurrent washing system for washing. Figure 2 It should be noted that Figure 2 This is an example of a four-stage series countercurrent washing, and is not intended to limit the number and position of adsorption zones, desorption zones, and washing columns.
[0038] Specifically, the adsorbent is a titanium-based adsorbent, and its components are lithium metatitanate (Li2TiO3) or lithium titanate (Li4Ti5O 12) or a mixture of the two. The salt lake brine is an alkaline brine with a pH>7, including alkaline sodium sulfate subtype salt lake brine, carbonate brine and lithium precipitation mother liquor. The lithium content in the alkaline brine with a pH>7 is 100mg / L-2000mg / L, the sodium content is 1-150g / L, the potassium content is 0.1g / L-35g / L, and the magnesium content is 0.1g / L-10g / L. By strengthening the adsorption conditions, the adsorption capacity reaches 4-12mg / g. After adsorption in the adsorption zone 31, the lithium content in the tail brine is 1mg / L-100mg / L, the sodium content is 1-150g / L, the potassium content is 0.1g / L-35g / L, and the magnesium content is 0.1g / L-10g / L.
[0039] S2, clean water or a solution of clean water with diluted acid added enters the first-stage washing column 27, and the adsorption column is subjected to multi-stage countercurrent washing, and the co-adsorbed elements such as sodium, potassium, and magnesium are eluted while washing the adsorbent. The washing liquid flowing out of each stage enters a separate washing liquid buffer tank 35-37, and after adding diluted acid to adjust the acid concentration, it enters the next-stage washing column. The washing liquid flowing out of the last-stage washing column 30 is sent to the adsorption tail brine tank 38 through a pipeline and returns to the salt lake;
[0040] For example, dilute acid is added from the dilute acid storage tank 33 to the clean water storage tank 34, the mixed solution flows into the first-stage washing column 27 and then into the first-stage washing liquid buffer tank 35, dilute acid is added thereto and then flows into the second-stage washing column 28, the operation is repeated until the washing liquid flows out of the last-stage washing column 30, and the washing liquid flows into the tail brine tank 28, mixes with the tail brine, and then returns to the salt lake.
[0041] The clean water described in step S2 includes surface river water, groundwater, softened water, membrane desalted water, and pure water. The dilute acid added to the clean water and each level of washing liquid is dilute hydrochloric acid or dilute sulfuric acid, which can be concentrated hydrochloric acid or an aqueous solution prepared by adding concentrated hydrochloric acid to water, or it can be dilute sulfuric acid or dilute hydrochloric acid solution produced by other processes such as bipolar membrane electrodialysis. The washing temperature is 1-50°C. The series number of multi-stage countercurrent washing is 2-6, and the flow rate is 1-10BV / h. The amount of clean water is 0.6-5BV, which is determined according to the impurity content of the brine, the number of countercurrent washing stages and the water balance requirements. After the acid is added, H at the inlet of each washing column + The arithmetic sum of the concentrations is 0.02-0.1 mol / L, distributed according to the order.
[0042] like Figure 2 As shown, when four-stage countercurrent washing is used, the H + The concentration is 0-0.05 mol / L. When the washing liquid flowing out of the first-stage washing column 27 flows into the second-stage washing column 28 after adding dilute acid, H +The concentration is 0.01-0.06mol / L. The washing liquid flowing out of the second-stage washing column flows into the third-stage washing column after adding dilute acid. + The concentration is 0.01-0.06mol / L. The washing liquid flowing out of the third-stage washing column flows into the fourth-stage washing column after adding dilute acid for 30 hours. + The concentration is 0-0.05mol / L.
[0043] The method of adding dilute acid is to connect a dilute acid adding pipe to the washing liquid delivery pipeline for online addition, and to measure the pH of the washing liquid entering the adsorption column through an online pH meter and flow meter. + The washing liquid and the dilute acid can also be added from the top of the adsorption column at the same time, and the upper liquid surface is used for mixing. The H in the mixed washing liquid is controlled by the flow rate of the washing liquid and the dilute acid. + concentration.
[0044] The liquid flow direction of the washing column includes top-in and bottom-out, bottom-in and top-out, or different arrangements and combinations of the two flow directions connected between different washing columns.
[0045] S3, the washed adsorption column is moved to the desorption zone 32 for desorption. In this embodiment, the desorption zone 32 has desorption columns 19-26. The obtained lithium-rich desorption liquid is concentrated and impurities are removed to prepare lithium hydroxide monohydrate or lithium carbonate products.
[0046] Example 1
[0047] The lithium-containing brine used in this embodiment is sodium sulfate subtype salt lake brine, and its composition is shown in Table 1.
[0048] Table 1
[0049] Components Li Na K Ca Mg Na / Li pH Content g / L 0.27 17.21 2.91 0.03 1.05 63.74 9.14
[0050] Adsorption: The brine used enters the adsorption zone of the continuous separation device, which is filled with titanium adsorbents, the main components of which are lithium metatitanate (Li2TiO3) and lithium titanate (Li4Ti5O 12 ) is mixed to adsorb lithium-containing brine, and the tail brine flowing out of the adsorption zone is returned to the salt lake. The composition of the tail brine is shown in Table 2.
[0051] Table 2
[0052] Components Li Na K Ca Mg Content g / L 0.03 17.02 2.83 0.01 0.95
[0053] Washing: The loaded adsorption column is washed using a 4-stage countercurrent washing method, with a water volume of 1BV, a washing flow rate of 7.5BV / h, and a temperature of 10°C. Clean water flows from top to bottom through the first-stage washing column and enters the first-stage washing liquid buffer tank. 1.6mol / L dilute hydrochloric acid is added to the first-stage washing liquid buffer tank to make the H+ The concentration is maintained at 0.04 mol / L. The first-stage washing liquid after acid supplementation flows from top to bottom through the second-stage washing column and enters the second-stage washing liquid buffer tank. 1.6 mol / L dilute hydrochloric acid is added to the second-stage washing liquid buffer tank to make the H + The concentration is maintained at 0.02mol / L. The second-stage washing liquid after acid supplementation flows from bottom to top through the third-stage washing column and enters the third-stage washing liquid buffer tank. 1.6mol / L dilute hydrochloric acid is added to the third-stage washing liquid buffer tank to make the H + The concentration is maintained at 0.01 mol / L. The third-stage washing liquid after acid supplementation flows from bottom to top through the fourth-stage washing column, and the washing liquid enters the tail brine tank.
[0054] Desorption: The cleaned adsorption column enters the desorption zone and is desorbed using a 2BV volume of 0.25mol / L hydrochloric acid solution to obtain a lithium-rich desorption solution. The desorption solution is concentrated and impurities are removed by membrane, and monohydrate lithium hydroxide can be prepared by MVR.
[0055] The components of the washing liquid and desorption liquid at each level are shown in Table 3.
[0056] Table 3
[0057]
[0058] Comparative Example 1
[0059] The brine composition, adsorption conditions, washing method and desorption conditions are the same as those in Example 1, except that no acid is added when four-stage countercurrent series washing is performed with clean water. The composition of each stage of washing liquid and desorption liquid is shown in Table 4.
[0060] Table 4
[0061]
[0062] Table 5
[0063]
[0064] The comparison of the desorption liquid components in Example 1 and Comparative Example 1 is shown in Table 5. As can be seen from the table, by applying the method of Example 1, the adsorbent is washed by adding acid during the countercurrent washing process, which can greatly reduce the sodium and potassium contents in the desorption liquid and slightly reduce the magnesium content in the desorption liquid. The Li / Na in the desorption liquid is increased from 1.89 to 3.62, and the elution rates of sodium and potassium are 45.6% and 65.0% respectively, while the lithium elution rate is only 1.05%.
[0065] Example 2
[0066] The lithium-containing brine used in this embodiment is an alkaline salt lake brine, and its composition is shown in Table 6.
[0067] Table 6
[0068] Components Li Na K Ca Mg Na / Li pH Content g / L 0.16 71.9 7.4 0.10 4.21 319 7.82
[0069] Adsorption: The brine used enters the adsorption zone of the continuous separation device, which is filled with titanium adsorbents, the main components of which are lithium metatitanate (Li2TiO3) and lithium titanate (Li4Ti5O 12 ) mixture, adsorb the lithium-containing brine, and the tail brine flowing out of the adsorption area returns to the salt lake. The tail brine composition is shown in Table 7. The sodium content in the tail brine is high, so it needs to enter the washing area to wash away the entrained brine in the column.
[0070] Table 7
[0071] Components Li Na K Ca Mg Content g / L 0.02 71.6 7.21 0.06 3.97
[0072] Washing: Use 3-stage series washing. Add H + The concentration of dilute sulfuric acid is 1.4 mol / L, so that the H + The concentration reaches 0.02mol / L, and the clean water flows from bottom to top through the first-stage washing column and enters the first-stage washing liquid buffer tank. The water volume is 1.3BV, and H is added to the first-stage washing liquid buffer tank. + The concentration of dilute sulfuric acid is 1.4 mol / L, so that H + The concentration reaches 0.03 mol / L. The first-stage washing liquid after acid supplementation flows from bottom to top through the second-stage washing column and enters the second-stage washing liquid buffer tank. H + The concentration of dilute sulfuric acid is 1.4 mol / L, so that H + The concentration reaches 0.01 mol / L. The second-stage washing liquid after acid supplementation flows from bottom to top through the third-stage washing column and enters the tail brine tank. The water temperature of the washing process is 5°C, and the washing flow rate is 8.67 BV / h.
[0073] Desorption: The cleaned adsorption column enters the desorption zone and is desorbed using 0.25 mol / L hydrochloric acid solution to obtain a lithium-rich qualified solution. The qualified solution is concentrated and impurity-removed, and lithium hydroxide monohydrate can be prepared through MVR.
[0074] The components of each level of washing liquid and desorption liquid are shown in Table 8.
[0075] Table 8
[0076]
[0077] Comparative Example 2
[0078] The brine composition, adsorption conditions, washing method and desorption conditions in this comparative example are the same as those in Example 2, except that when the adsorption column is washed after adsorption, no dilute sulfuric acid is added to the clean water and the washing liquid at each level. The composition of the washing liquid at each level and the desorption liquid are shown in Table 9.
[0079] Table 9
[0080]
[0081]
[0082] Table 10
[0083]
[0084] The comparison of the desorption liquid components in Example 2 and Comparative Example 2 is shown in Table 10. As can be seen from the table, by applying the method of Example 2, washing the adsorbent in clean water and washing liquid at each level by adding acid in a stepwise manner, the sodium and potassium contents in the desorption liquid can be greatly reduced, and the magnesium content in the desorption liquid can be slightly reduced. The Li / Na in the desorption liquid is increased from 1.61 to 3.73, and the elution rates of sodium and potassium are 53.3% and 73.1% respectively, while the lithium loss rate is only 1.51%.
[0085] Example 3
[0086] The lithium-containing solution used in this embodiment is a lithium precipitation mother solution, and its composition is shown in Table 11.
[0087] Table 11
[0088]
[0089] Adsorption: The brine used enters the adsorption zone of the continuous separation device, which is filled with titanium adsorbents, the main components of which are lithium metatitanate (Li2TiO3) and lithium titanate (Li4Ti5O 12 ) mixture, adsorb the lithium-containing brine, and the tail brine flowing out of the adsorption area returns to the salt lake. The tail brine composition is shown in Table 12. The sodium content in the tail brine is high, so it needs to enter the washing area to wash away the entrained brine in the column.
[0090] Table 12
[0091] Components Li Na K Content g / L 0.08 116.3 7.55
[0092] Washing: Use 6-stage series washing. No dilute hydrochloric acid is added to the clean water, that is, H + The concentration is 0mol / L, and the clean water flows from top to bottom through the first-stage washing column and enters the first-stage washing liquid buffer tank. The water volume is 0.8BV, and H is added to the first-stage washing liquid buffer tank. +The concentration is 1.5 mol / L dilute hydrochloric acid, so that H + The concentration reaches 0.01mol / L. The first-stage washing liquid after acid supplementation flows from top to bottom through the second-stage washing column and enters the second-stage washing liquid buffer tank. H + The concentration is 1.5 mol / L dilute hydrochloric acid, so that H + The concentration reaches 0.015mol / L. The second-stage washing liquid after acid supplementation flows from top to bottom through the third-stage washing column and enters the third-stage washing liquid buffer tank. Dilute hydrochloric acid with a H+ concentration of 1.5mol / L is added to the third-stage washing liquid buffer tank to make the H+ in the third-stage washing liquid + The concentration reaches 0.015 mol / L. The third-stage washing liquid after acid supplementation flows from bottom to top through the fourth-stage washing column and enters the fourth-stage washing liquid buffer tank. H + The concentration is 1.5 mol / L dilute hydrochloric acid, so that the H + The concentration reaches 0.02mol / L. The fourth-stage washing liquid after acid supplementation flows from bottom to top through the fifth-stage washing column and enters the fifth-stage washing liquid buffer tank. The fifth-stage washing liquid does not add dilute hydrochloric acid, that is, the H in the sixth-stage washing column + The concentration is 0 mol / L. The washing liquid enters the tail brine tank. The water temperature of the washing process is 20°C, and the washing flow rate is 4.8 BV / h.
[0093] Desorption: The cleaned adsorption column enters the desorption zone and is desorbed using 0.25 mol / L hydrochloric acid solution to obtain a lithium-rich qualified solution. The qualified solution is concentrated and impurity-removed, and lithium hydroxide monohydrate can be prepared through MVR.
[0094] The components of each level of washing liquid and desorption liquid are shown in Table 13.
[0095] Table 13
[0096]
[0097] Comparative Example 3
[0098] The brine composition, adsorption conditions, washing method and desorption conditions in this comparative example are the same as those in Example 3, except that when the adsorption column is washed after adsorption, no dilute hydrochloric acid is added to the clean water and the washing liquid at each level. The composition of the washing liquid at each level and the desorption liquid are shown in Table 14.
[0099] Table 14
[0100]
[0101]
[0102] Table 15
[0103]
[0104] The comparison of the desorption liquid components in Example 3 and Comparative Example 3 is shown in Table 15. As can be seen from the table, by applying the method of Example 3, washing the adsorbent in clean water and washing liquid at each level by stepwise acid addition, the sodium and potassium contents in the desorption liquid can be greatly reduced, and the magnesium content in the desorption liquid can be slightly reduced. The Li / Na in the desorption liquid is increased from 1.97 to 3.81, and the elution rates of sodium and potassium are 48.6% and 43.6% respectively, while the lithium loss rate is only 1.72%.
[0105] Example 4
[0106] The adsorption and desorption experiments were carried out using the brines shown in Table 1.
[0107] Adsorption: The brine used enters the adsorption zone of the continuous separation device, which is filled with titanium adsorbents, the main components of which are lithium metatitanate (Li2TiO3) and lithium titanate (Li4Ti5O 12 The adsorption temperature is 5°C, the halogen flow rate is 12BV, and the feed flow rate is 12BV / h.
[0108] Desorption: No diluted acid was added to the lithium-loaded adsorbent during washing. After washing, 0.3 mol / L hydrochloric acid solution was used for desorption at a flow rate of 12 BV / h and a desorption temperature of 40°C.
[0109] Example 5
[0110] The difference from Example 4 is that the halogen intake is adjusted to 24 BV, and the other experimental conditions and methods are the same as those of Example 4.
[0111] Example 6
[0112] The difference from Example 4 is that the halogen intake is adjusted to 36 BV, and the other experimental conditions and methods are the same as those of Example 4.
[0113] Example 7
[0114] The difference from Example 4 is that the halogen intake is adjusted to 48 BV, and the other experimental conditions and methods are the same as those of Example 4.
[0115] Table 16
[0116]
[0117] The desorption liquid composition of Examples 4-7 is shown in Table 16. As the halogen flow rate increases from 12 BV to 48 BV, the lithium concentration in the desorption liquid increases significantly, the sodium and potassium contents in the desorption liquid remain relatively stable, Li / Na increases from 1.25 to 2.39, and the magnesium content increases only slightly. Therefore, the adsorption capacity of the adsorbent for lithium can be increased by increasing the amount of halogen.
[0118] By comparing the above examples, it can be found that the method for extracting lithium from salt lake brine and controlling the impurity content of the desorption liquid in this embodiment is innovative. In the multi-stage countercurrent washing stage of the loaded adsorbent, the effective washing of the brine entrained in the adsorption column and the effective elution of the sodium, potassium and magnesium co-adsorbed on the adsorbent are organically combined by adding acid in the form of additional acid in the multi-stage countercurrent washing stage of the loaded adsorbent. The amount of clean water used is 0.5-2BV, which can greatly reduce the sodium and potassium content in the desorption liquid, and the magnesium content is also slightly reduced, and the lithium loss is controlled at a low level. The significant reduction in the impurity content in the desorption liquid can reduce the burden of impurity removal in the subsequent concentration process, reduce the power consumption of electrodialysis, and greatly improve the recovery rate and product quality of MVR and multi-effect evaporation crystallization to produce monohydrate lithium hydroxide. It can help enterprises save energy, reduce consumption, reduce costs and increase efficiency, and has great social and economic benefits.
[0119] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A method for extracting lithium from salt lake brine and controlling the impurity content of the desorption solution, characterized in that: The specific process is: S1. Use a continuous ion exchange device to adsorb lithium in lithium-containing salt lake brine passing through an adsorption column after loading a lithium-extracting adsorbent. The tail brine after adsorption flows out of the continuous ion exchange device and returns to the salt lake. The loaded adsorption column carrying brine enters the last stage of a multi-stage countercurrent washing system for washing. S2, clean water or a solution of clean water with diluted acid added enters the first-stage washing column, and the load adsorption column is subjected to multi-stage countercurrent washing, and the co-adsorbed sodium, potassium and magnesium elements are eluted while washing the load adsorption column; the washing liquid flowing out of each washing column is supplemented with diluted acid to adjust the acid concentration and then enters the next-stage washing column, and the washing liquid flowing out of the last-stage washing column is returned to the salt lake through a pipeline; When the loaded adsorption column is washed using a 4-stage countercurrent washing method, the water volume is 1BV, the washing flow rate is 7.5BV / h, and the temperature is 10°C; the clean water flows from top to bottom through the first-stage washing column and enters the first-stage washing liquid buffer tank. 1.6mol / L dilute hydrochloric acid is added to the first-stage washing liquid buffer tank to make the H in the washing liquid in the first-stage washing liquid buffer tank + The concentration is maintained at 0.04mol / L; the first-stage washing liquid after acid supplementation flows from top to bottom through the second-stage washing column and enters the second-stage washing liquid buffer tank, and 1.6mol / L dilute hydrochloric acid is added to the second-stage washing liquid buffer tank to make the H + The concentration is maintained at 0.02mol / L; the second-stage washing liquid after acid supplementation flows from bottom to top through the third-stage washing column and enters the third-stage washing liquid buffer tank, and 1.6mol / L dilute hydrochloric acid is added to the third-stage washing liquid buffer tank to make the H + The concentration is maintained at 0.01mol / L; the third-stage washing liquid after acid supplementation flows from bottom to top through the fourth-stage washing column, and the washing liquid enters the tail brine tank; When washing the loaded adsorption column using a three-stage series method, add H + The concentration of dilute sulfuric acid is 1.4 mol / L, so that the H + The concentration reaches 0.02mol / L; the clean water flows from bottom to top through the first-stage washing column and enters the first-stage washing liquid buffer tank. The water volume is 1.3BV, and H is added to the first-stage washing liquid buffer tank. + The concentration of dilute sulfuric acid is 1.4 mol / L, so that H + The concentration reaches 0.03 mol / L; the first-stage washing liquid after acid supplementation flows from bottom to top through the second-stage washing column and enters the second-stage washing liquid buffer tank, and H is added to the second-stage washing liquid buffer tank. + The concentration of dilute sulfuric acid is 1.4 mol / L, so that H + The concentration reaches 0.01mol / L; the second-stage washing liquid after acid supplementation flows from bottom to top through the third-stage washing column and enters the tail brine tank; the water temperature of the washing process is 5°C, and the washing flow rate is 8.67BV / h; When the loaded adsorption column is washed in a 6-stage series mode, no dilute hydrochloric acid is added to the clean water, that is, H + The concentration is 0mol / L, and the clean water flows from top to bottom through the first-stage washing column and enters the first-stage washing liquid buffer tank. The water volume is 0.8BV, and H is added to the first-stage washing liquid buffer tank. + The concentration is 1.5 mol / L dilute hydrochloric acid, so that H + The concentration reaches 0.01mol / L; the first-stage washing liquid after acid supplementation flows from top to bottom through the second-stage washing column and enters the second-stage washing liquid buffer tank, and H is added to the second-stage washing liquid buffer tank. + The concentration is 1.5 mol / L dilute hydrochloric acid, so that H + The concentration reaches 0.015mol / L; the second-stage washing liquid after acid supplementation flows from top to bottom through the third-stage washing column and enters the third-stage washing liquid buffer tank, and dilute hydrochloric acid with a H+ concentration of 1.5mol / L is added to the third-stage washing liquid buffer tank to make the H+ in the third-stage washing liquid + The concentration reaches 0.015mol / L; the third-stage washing liquid after acid supplementation flows from bottom to top through the fourth-stage washing column and enters the fourth-stage washing liquid buffer tank, and H is added to the fourth-stage washing liquid buffer tank. + The concentration is 1.5 mol / L dilute hydrochloric acid, so that the H + The concentration reaches 0.02mol / L; the fourth-stage washing liquid after acid supplementation flows from bottom to top through the fifth-stage washing column and enters the fifth-stage washing liquid buffer tank. The fifth-stage washing liquid does not add dilute hydrochloric acid, that is, it enters the H in the sixth-stage washing column. + The concentration is 0 mol / L; the washing liquid enters the tail brine tank; the water temperature of the washing process is 20°C, and the washing flow rate is 4.8 BV / h; S3. The washed adsorption column is moved to a desorption zone for desorption to obtain a lithium-rich desorption solution, and the lithium-rich desorption solution is concentrated and impurities are removed to prepare lithium hydroxide monohydrate or lithium carbonate products.
2. The method according to claim 1, characterized in that In step S1, when lithium in lithium-containing salt lake brine passing through the adsorption column is adsorbed, the lithium adsorption capacity of the adsorbent is increased to 4-21 mg / g by increasing the amount of brine input.
3. The method according to claim 1, characterized in that: In step S1, the lithium extraction adsorbent is a titanium adsorbent, such as lithium metatitanate Li2TiO3 and lithium titanate Li4Ti5O 12 One or a mixture of two.
4. The method according to claim 1, characterized in that: In step S1, the lithium-containing salt lake brine is an alkaline brine with a pH value greater than 7, a lithium content of 100 mg / L-2000 mg / L, a sodium content of 1-150 g / L, a potassium content of 0.1 g / L-35 g / L, and a magnesium content of 0.1 g / L-10 g / L; the alkaline brine includes one or more of alkaline sodium sulfate subtype salt lake brine, carbonate brine, and lithium precipitation mother liquor.
5. The method according to claim 1, characterized in that In step S2, the clean water includes one or more of surface river water, groundwater, softened water, membrane-treated desalted water, and pure water.
6. The method according to claim 1, characterized in that In step S2, the dilute acid is dilute hydrochloric acid or dilute sulfuric acid.
7. The method according to claim 1, characterized in that In step S2, the dilute acid added to the clean water and each level of washing liquid is concentrated hydrochloric acid or an aqueous solution prepared by adding concentrated hydrochloric acid to water, or a dilute sulfuric acid or dilute hydrochloric acid solution produced by a bipolar membrane electrodialysis process.
8. The method according to claim 1, characterized in that In step S2, the method of adding dilute acid is as follows: the washing liquid flowing out of each stage enters a separate buffer tank, and dilute acid is added to adjust the acid concentration before entering the next washing column; or a dilute acid adding pipe is connected to the washing liquid delivery pipeline to add dilute acid online, and the washing liquid pH at the washing column inlet is measured by an online pH meter and flow meter. + The concentration can be controlled by adding the washing liquid and the dilute acid from the top of the adsorption column at the same time, and the H in the washing liquid after mixing can be controlled by the flow rate of the washing liquid and the dilute acid. + concentration.