A PBS-based modified film for biodegradable garbage bags
PBS-based modified film prepared by blending modified PBS particles with luteolin and PBAT solves the problems of high brittleness and high production costs in traditional PBS garbage bags, improves the mechanical properties and biodegradable properties of the materials, and achieves environmental protection garbage bag application.
Patent Information
- Application Number
- CN202211689039.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Traditional PBS garbage bags have limited their promotion and application due to their high brittleness and high production costs, and have caused pollution to the environment.
Modified PBS pellets are blended with luteolin and PBAT, and PBS-based modified film is prepared through a twin-screw extruder and a film blowing mechanism. Luteolin is used as a natural antioxidant and nucleating agent, so PBAT improves the flexibility of the material. and melting point to improve the mechanical properties of PBS.
It improves the mechanical properties and biodegradable properties of PBS films, reduces production costs, enhances the environmental protection and degradability of the materials, and reduces environmental pollution.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of degradable films, and in particular relates to a PBS-based modified film for biodegradable garbage bags. Background Art
[0002] Plastic garbage bags are indispensable in people's lives. They have no irritating odor and are easy and quick to use, which provides convenience for daily life. However, traditional garbage bags are difficult to degrade and are used in large quantities, causing very serious environmental pollution and greenhouse effect problems. Therefore, the promotion and application of biodegradable garbage bags is imperative, and it is also one of the effective ways to develop green materials. Biodegradable materials are polymer materials that have good performance during use and can be naturally degraded after use. This material can significantly reduce environmental pollution. Among various types of degradable polymer materials, polybutylene succinate (PBS) is a degradable material with excellent comprehensive performance. However, since PBS has a crystallinity of 40-60%, a relatively regular structure, brittleness, and a high production cost, its promotion and application are limited. Summary of the invention
[0003] The object of the present invention is to provide a biodegradable PBS-based modified film for garbage bags, so as to solve the problems of high brittleness and high production cost of PBS in the background technology.
[0004] The purpose of the present invention can be achieved by the following technical solutions:
[0005] A PBS-based modified film for biodegradable garbage bags, comprising the following raw materials in parts by weight: 96.95-108.05 parts of modified PBS particles, 7.2-10.8 parts of luteolin, and 26.16-39.24 parts of PBAT particles;
[0006] The preparation process includes the following steps:
[0007] Step A1, heating the modified PBS particles to 150-160° C., and after completely melting, adding luteolin, mixing evenly, and then melt-extruding and granulating with a twin-screw extruder to obtain PBS composite material particles;
[0008] Step A2, drying the PBS composite material particles and the PBAT particles in a drying oven at 70-90° C. for 18-20 hours to reach a constant weight, adding the dried PBS composite material particles and the PBAT particles into a torque rheometer for melt blending, and the modified PBS particles as a compatibilizer can effectively improve the interfacial compatibility of the polymer, thereby improving the mechanical properties of the material;
[0009] Step A3: extruding the blend and cooling and granulating the blend to obtain the desired blend particles, and feeding the blend particles into a film blowing machine to blow into a film to obtain a PBS-based modified film.
[0010] Furthermore, the preparation of the modified PBS particles comprises the following steps:
[0011] Maleic anhydride, dicumyl peroxide and PBS are mixed, and then melt-extruded and granulated at 155-165° C. using a twin-screw extruder to obtain modified PBS particles, wherein dicumyl peroxide is used as an initiator to initiate the polymerization reaction of maleic anhydride grafted PBS.
[0012] Furthermore, the mass ratio of maleic anhydride, dicumyl peroxide and PBS is 1.5-2.5:0.45-0.55:95-105.
[0013] Furthermore, the luteolin is an extract from honeysuckle leaves. Honeysuckle is selected because honeysuckle leaves are large in quantity, easy to collect and obtain, and the content of luteolin in honeysuckle leaves is relatively high, but they are often wasted as a by-product of honeysuckle.
[0014] Furthermore, the extraction of luteolin comprises the following steps:
[0015] The dried and crushed honeysuckle leaves are soaked in a mixed solution of methanol and sodium hydroxide for 10-12 hours, then ultrasonically extracted and heated at 50-65°C for 30-40 minutes, filtered and concentrated, and then filtered with a microporous filter membrane to obtain luteolin.
[0016] Furthermore, the usage ratio of the honeysuckle leaves, methanol and sodium hydroxide solution is 0.5-1g:10-25mL:1-5mL, and the mass fraction of the sodium hydroxide solution is 20-30%.
[0017] Beneficial effects of the present invention:
[0018] The present invention prepares PBS composite material particles by introducing luteolin extracted from honeysuckle leaves into modified PBS particles. Luteolin is a natural antioxidant with a wide source and low price. Luteolin added to the composite material can act as a heterogeneous component to induce PBS, form heterogeneous nucleation points at the contact surface, and play the role of a nucleating agent. The high-efficiency nucleating agent can effectively change the crystal size of PBS, increase the crystallization speed, refine the structure, and improve the smoothness and transparency of the product appearance.
[0019] The polybutylene adipate terephthalate (PBAT) used in the present invention has the flexibility of a long methylene chain and the rigidity of an aromatic ring. The rigid aromatic component can increase the melting point of PBS and improve the mechanical properties of PBS without affecting the biodegradability of PBS, while the flexible aliphatic component can improve the brittleness and degradation properties of PBS.
[0020] The present invention adopts modified PBS particles as the main raw material. Since the maleic anhydride grafted PBS particles can increase the interfacial compatibility of the polymer, the melting temperature, tensile strength and elongation at break of the composite material are improved. The garbage bag prepared by using the composite material has the advantages of being environmentally friendly and biodegradable, and therefore does not cause a burden on the environment. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Example 1
[0023] A method for preparing modified PBS particles comprises the following steps:
[0024] 1.5 parts of maleic anhydride, 0.45 parts of dicumyl peroxide and 95 parts of PBS were mixed, and then melt-extruded and granulated at 155° C. using a twin-screw extruder to prepare modified PBS particles.
[0025] Example 2
[0026] A method for preparing modified PBS particles comprises the following steps:
[0027] 2 parts of maleic anhydride, 0.5 parts of dicumyl peroxide and 100 parts of PBS were mixed, and then melt-extruded and granulated at 160° C. using a twin-screw extruder to obtain modified PBS particles.
[0028] Example 3
[0029] A method for preparing modified PBS particles comprises the following steps:
[0030] 2.5 parts of maleic anhydride, 0.55 parts of dicumyl peroxide and 105 parts of PBS were mixed, and then melt-extruded and granulated at 165° C. using a twin-screw extruder to prepare modified PBS particles.
[0031] Example 4
[0032] A luteolin is prepared by the following steps:
[0033] 0.5 g of dried and crushed honeysuckle leaves were soaked in a mixed solution of 10 mL of methanol and 1 mL of 20% sodium hydroxide by mass for 10 h, then ultrasonically extracted and heated at 50°C for 30 min, filtered and concentrated, and then filtered with a 0.45 μm microporous filter membrane to obtain luteolin.
[0034] Example 5
[0035] A luteolin is prepared by the following steps:
[0036] 0.75 g of dried and crushed honeysuckle leaves were soaked in a mixed solution of 17.5 mL of methanol and 3 mL of 25% sodium hydroxide by mass for 11 hours, then ultrasonically extracted and heated at 57.5°C for 35 minutes, filtered and concentrated with a 0.45 μm microporous filter membrane to obtain luteolin.
[0037] Example 6
[0038] A luteolin is prepared by the following steps:
[0039] 1 g of dried and crushed honeysuckle leaves was soaked in a mixed solution of 25 mL of methanol and 5 mL of 30% sodium hydroxide by mass for 12 hours, then ultrasonically extracted and heated at 65°C for 40 minutes, filtered and concentrated with a 0.45 μm microporous filter membrane to obtain luteolin.
[0040] Example 7
[0041] A PBS-based modified film for biodegradable garbage bags is prepared by the following steps:
[0042] Step A1, heating 96.95 parts of modified PBS particles to 150° C., and after completely melting, adding 7.2 parts of luteolin, mixing evenly, and then melt-extruding and granulating using a twin-screw extruder to obtain modified PBS composite material particles;
[0043] Step A2, drying 87.2 parts of PBS composite particles and 26.16 parts of PBAT particles in a 70° C. oven for 20 hours to reach constant weight, and adding the dried PBS composite particles and PBAT particles into a torque rheometer for melt blending;
[0044] Step A3: extruding the blend and cooling and granulating the blend to obtain the desired blend particles, and feeding the blend particles into a film blowing machine to blow into a film to obtain a PBS-based modified film.
[0045] Example 8
[0046] A PBS-based modified film for biodegradable garbage bags is prepared by the following steps:
[0047] Step A1, heating 102.5 parts of modified PBS particles to 155° C., and after completely melting, adding 9 parts of luteolin, mixing evenly, and then melt-extruding and granulating with a twin-screw extruder to obtain PBS composite material particles;
[0048] Step A2, drying 109 parts of PBS composite particles and 27.7 parts of PBAT particles in an oven at 80° C. for 21 hours to reach constant weight, and adding the dried PBS composite particles and PBAT particles into a torque rheometer for melt blending;
[0049] Step A3: extruding the blend and cooling and granulating the blend to obtain the desired blend particles, and feeding the blend particles into a film blowing machine to blow into a film to obtain a PBS-based modified film.
[0050] Example 9
[0051] A PBS-based modified film for biodegradable garbage bags is prepared by the following steps:
[0052] Step A1, heating 108.05 parts of modified PBS particles to 160° C., and after completely melting, adding 10.8 parts of luteolin, mixing evenly, and then melt-extruding and granulating with a twin-screw extruder to obtain PBS composite material particles;
[0053] Step A2, drying 109 parts of PBS composite particles and 39.24 parts of PBAT particles in a 90° C. oven for 22 hours to reach constant weight, and adding the dried PBS composite particles and PBAT particles into a torque rheometer for melt blending;
[0054] Step A3: extruding the blend and cooling and granulating the blend to obtain the desired blend particles, and feeding the blend particles into a film blowing machine to blow into a film to obtain a PBS-based modified film.
[0055] Comparative Example 1
[0056] Compared with Example 7, PBAT was not added in the preparation process of the PBS-based modified film for biodegradable garbage bags in this comparative example. The remaining steps and parameters were the same, and this comparative example will not be repeated. Finally, a PBS-based modified film for biodegradable garbage bags was obtained.
[0057] Comparative Example 2
[0058] Compared with Example 8, luteolin was not added in the preparation process of the PBS-based modified film for biodegradable garbage bags in this comparative example. The remaining steps and parameters were the same and will not be repeated in this comparative example. Finally, a PBS-based modified film for biodegradable garbage bags was obtained.
[0059] First, the samples were subjected to DSC test. The samples of Example 7 to Example 9 and Comparative Example 1 to Comparative Example 2 were weighed and pressed into sample sheets in a sample tray, and then tested under the protection of high-purity nitrogen. The heating rate was set to 10°C / min, from room temperature 23°C to 200°C, and the cooling rate was also set to 10°C / min, from 200°C to -50°C, and finally the heating rate was raised to 200°C again at a heating rate of 10°C / min;
[0060] The samples were then subjected to mechanical property tests. Referring to GB / TI3022-91 standard, the samples prepared in Examples 7-9 and Comparative Examples 1-2 were cut into dumbbell shapes and tested at a tensile speed of 10 mm / min to determine and calculate the elongation at break of the modified PBS samples. The results are shown in Table 1:
[0061] Table 1
[0062] project Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Elongation at break / % 394.6 414.6 434.6 77.7 380.7 Tm / ℃ 115.71 117.2 116.62 116.7 105.3
[0063] It can be seen from Table 1 that, compared with Comparative Example 1 and Comparative Example 2, the PBS-based modified films for biodegradable garbage bags prepared in Examples 7 to 9 have higher elongation at break and higher melting points. This is because PBAT and luteolin are added to modify PBS during the preparation process of Examples 7 to 9. Luteolin added to the composite material can act as a heterogeneous component to induce PBS, forming heterogeneous nucleation points at its contact surface, playing the role of a nucleating agent, causing the PBS polymer to crystallize due to spatial hindrance, ensuring the degradable properties of the composite material while improving the comprehensive performance of the composite material. PBAT has the flexibility of a long methylene chain and the rigidity of an aromatic ring, has good ductility and high flexibility, and has a high melt flow rate. Modifying PBS with PBAT can significantly improve the toughness of PBS.
[0064] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A PBS-based modified film for biodegradable garbage bags, characterized in that: The raw materials include, by weight: 96.95-108.05 parts of modified PBS particles, 7.2-10.8 parts of luteolin, and 26.16-39.24 parts of PBAT particles; The PBS-based modified film is prepared by the following steps: Step A1, heating the modified PBS particles until they are completely melted, adding luteolin, mixing evenly, and then melt-extruding and granulating them using a twin-screw extruder to obtain PBS composite material particles; Step A2, drying the PBS composite material particles and the PBAT particles in an oven at 70-90° C. to constant weight, adding the dried modified PBS particles and PBAT particles into a torque rheometer for melt blending to obtain a blend; Step A3, extruding the blend and cooling and granulating to obtain desired blend particles, and putting the blend particles into a film blowing machine to blow into a film to obtain a PBS-based modified film; The preparation of the modified PBS particles comprises the following steps: Maleic anhydride, dicumyl peroxide and PBS are mixed, and then melt-extruded and granulated at 155-165° C. using a twin-screw extruder to obtain modified PBS particles; The luteolin is an extract of honeysuckle leaves, which is prepared by the following steps: The dried and crushed honeysuckle leaves are soaked in a mixed solution of methanol and sodium hydroxide for 10-12 hours, then ultrasonically extracted at 50-65°C for 30-40 minutes, filtered and concentrated, and then filtered with a microporous filter membrane to obtain luteolin.
2. The PBS-based modified film for biodegradable garbage bags according to claim 1, characterized in that: The mass ratio of maleic anhydride, dicumyl peroxide and PBS is 1.5-2.5:0.45-0.55:95-105.
3. The PBS-based modified film for biodegradable garbage bags according to claim 1, characterized in that: The mass ratio of the honeysuckle leaves, methanol and sodium hydroxide solution is 0.5-1:10-25:1-5, and the mass fraction of the sodium hydroxide solution is 20-30%.
4. The PBS-based modified film for biodegradable garbage bags according to claim 1, characterized in that: In step A1, the modified PBS particles are heated to 150-160°C.