Method for forming image sensor and semiconductor device
By adopting a hybrid DTI structure in the image sensor, the isolation structure, dielectric liner and fill layer are used to achieve photoelectric isolation between pixels, which solves the optical crosstalk problem and improves the signal-to-noise ratio and image quality.
Patent Information
- Application Number
- CN202211106008.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-16
- Filing Date
- 2022-09-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-09
AI Technical Summary
The optical crosstalk between adjacent pixels in existing image sensors is serious, affecting the signal-to-noise ratio and image integrity.
Using a hybrid deep trench isolation (DTI) structure, the isolation structure, dielectric liner, conductive layer and fill layer are formed on the substrate to achieve photoelectric isolation of adjacent pixels, increasing quantum efficiency and reducing optical crosstalk.
It effectively improves the quantum efficiency and signal-to-noise ratio of the image sensor, reduces optical crosstalk, and improves image integrity.
Smart Images

Figure CN115831989B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to an image sensor pixel with a deep trench isolation structure. Background Art
[0002] Image sensors are now ubiquitous. An image sensor may include an array of pixels arranged in a two-dimensional manner. Each pixel includes a photodiode or other suitable photoelectric element. A microlens may be formed above the photodiode. The microlens focuses light onto the photodiode, which converts the light into an electrical signal. The electrical signal is output from the image sensor to other components of a host electronic device (e.g., a digital camera, cell phone, computer, security camera, automotive product, medical accessory, or other electronic device) to form an image.
[0003] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological advances in IC materials and design have produced several generations of ICs, each of which is smaller and more complex than the previous generation. The technology used to manufacture image sensors, such as complementary metal oxide semiconductor (CMOS) image sensor technology, is also constantly improving. The demand for higher resolution and lower power consumption has driven the trend of further miniaturization and integration of image sensors. The corresponding pixels in the image sensor are therefore reduced. This reduction process generally provides benefits by improving production efficiency and reducing associated costs. This reduction also increases the complexity of processing and manufacturing ICs. For example, as pixel size continues to decrease, optical crosstalk and interference between pixels may occur more frequently. Deep trench isolation (DTI) structures have been proposed to isolate pixels from each other. Although existing DTI structures are generally sufficient for their intended purposes, they are not completely satisfactory in all aspects. Summary of the invention
[0004] The embodiments of the present application provide a method for forming an image sensor and a semiconductor device to achieve photoelectric isolation of adjacent pixels in the image sensor, thereby improving quantum efficiency and reducing optical crosstalk. Therefore, the signal-to-noise ratio can be improved and the image integrity can be improved.
[0005] In a first aspect, an embodiment of the present application provides a method for forming an image sensor, comprising:
[0006] receiving a workpiece including a first isolation structure formed in a front side of a substrate;
[0007] forming a first trench extending through the first isolation structure and a portion of the substrate;
[0008] forming a dielectric liner to line the first trench;
[0009] after forming the dielectric liner, conformally depositing a conductive layer over the workpiece; and,
[0010] A filling layer is deposited over the conductive layer to fill the first trench.
[0011] In some embodiments, the refractive index of the conductive layer is greater than the refractive index of the fill layer.
[0012] In some embodiments, the conductive layer includes doped polysilicon, titanium nitride, aluminum, or tungsten.
[0013] In some embodiments, the fill layer includes silicon oxide, silicon nitride, or silicon carbide.
[0014] In some embodiments, it also includes:
[0015] forming an interconnect structure over the front side of the substrate, the interconnect structure comprising an interlayer dielectric layer and a conductive feature in the interlayer dielectric layer, wherein the conductive feature is electrically coupled to the conductive layer; and,
[0016] A bias voltage is applied to the conductive layer via the conductive member.
[0017] In some embodiments, depositing the fill layer includes:
[0018] conformally depositing a first fill layer over the conductive layer; and,
[0019] A second fill layer is conformally deposited over the first fill layer, wherein a composition of the second fill layer is different from a composition of the first fill layer.
[0020] In some embodiments, it also includes:
[0021] Etching back the conductive layer and the filling layer to form a second trench in the first trench;
[0022] depositing a dielectric layer over the workpiece to fill the second trench; and,
[0023] A planarization process is performed on the workpiece.
[0024] In some embodiments, the workpiece further comprises a protection layer formed over the front side of the substrate, wherein a top surface of the protection layer is coplanar with a top surface of the first isolation structure; and wherein performing the planarization process comprises: removing excess material on the protection layer.
[0025] In some embodiments, it also includes:
[0026] After depositing the dielectric fill layer, flipping the workpiece; and,
[0027] A planarization process is performed on a back side of the substrate to expose the filling layer, the back side of the substrate being opposite to the front side of the substrate.
[0028] In some embodiments, it also includes:
[0029] Before performing a planarization process on the back side of the substrate, a first photosensitive element and a second photosensitive element are formed in the substrate, wherein the first photosensitive element and the second photosensitive element are isolated from each other by a dielectric liner, a conductive layer and a filling layer.
[0030] In some embodiments, forming the dielectric liner includes:
[0031] Thermal oxidation of the workpiece;
[0032] After the conductive layer is deposited, a first portion of the conductive layer is in direct contact with the dielectric liner, and a second portion of the conductive layer is in direct contact with the first isolation structure.
[0033] In some embodiments, forming the dielectric liner includes:
[0034] performing a deposition process on the workpiece;
[0035] The conductive layer and the first isolation structure are separated by a dielectric liner.
[0036] In some embodiments, forming the first trench includes:
[0037] forming a patterned hard mask layer over the workpiece, the patterned hard mask layer comprising an opening exposing a portion of the first isolation structure; and,
[0038] An etching process is performed using the patterned hard mask layer as an etching mask to remove a portion of the first isolation structure and a portion of the substrate, wherein a portion of the substrate is located directly below a portion of the first isolation structure.
[0039] In a second aspect, an embodiment of the present application provides a method for forming an image sensor, including:
[0040] receiving a workpiece including a first isolation structure formed in a front side of a substrate;
[0041] forming a third trench extending through the first isolation structure and a portion of the substrate;
[0042] forming a doped region along the sidewalls and bottom surface of the third trench, the doped region including a dopant having the same doping polarity as the substrate;
[0043] After forming the doped region, forming a dielectric liner to line the third trench;
[0044] after forming the dielectric liner, conformally depositing a conductive layer over the workpiece; and,
[0045] A filling layer is deposited over the conductive layer to fill the third trench.
[0046] In a third aspect, an embodiment of the present application provides a semiconductor device, including:
[0047] a substrate having a front surface and a back surface;
[0048] A first photosensitive element and a second photosensitive element disposed in the substrate; and
[0049] an isolation structure extending through the substrate and disposed between the first photosensitive element and the second photosensitive element;
[0050] The isolation structure includes an upper portion and a lower portion located directly below the upper portion, wherein the upper portion is closer to the front surface than the lower portion, and wherein the lower portion includes:
[0051] a first dielectric layer extending from the upper portion to the backside surface;
[0052] a conductive layer surrounding the sidewall surface of the first dielectric layer; and,
[0053] A second dielectric layer surrounds the sidewall surface of the conductive layer, wherein the first dielectric layer and the second dielectric layer are separated by the conductive layer.
[0054] In some embodiments, the conductive layer is biased to a predetermined voltage.
[0055] In some embodiments, the conductive layer has a refractive index greater than a refractive index of the first dielectric layer.
[0056] In some embodiments, it also includes:
[0057] A first color filter disposed below the first photosensitive element; and
[0058] A second color filter is disposed below the second photosensitive element.
[0059] In some embodiments, the conductive layer includes doped polysilicon and the first dielectric layer includes silicon oxide.
[0060] In some embodiments, the lower portion further comprises:
[0061] a doped region surrounding a sidewall surface of the second dielectric layer;
[0062] The doping region includes a dopant having a first doping polarity, and the first photosensitive element and the second photosensitive element include another doping region having a second polarity opposite to the first doping polarity.
[0063] The method for forming an image sensor and the semiconductor device provided in the embodiments of the present application can achieve photoelectric isolation of adjacent pixels in the image sensor by forming a hybrid DTI structure, thereby improving quantum efficiency and reducing optical crosstalk. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] The present invention can be best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be emphasized that, in accordance with standard practice in the industry, the various components are not drawn to scale and are only used for illustrative purposes. In fact, the size of the various components may be arbitrarily increased or reduced for clarity of discussion.
[0065] Figure 1 is a flow chart of an exemplary method for manufacturing a semiconductor device having a deep trench isolation (DTI) structure according to various embodiments of the present application.
[0066] Figures 2 to 14 It is according to various aspects of this application that the workpiece is displayed according to Figure 1 A partial cross-sectional view of an embodiment of the method during manufacture is shown.
[0067] Fig.15 is a flow chart of another exemplary method for manufacturing a semiconductor device having a deep trench isolation (DTI) structure according to various embodiments of the present application.
[0068] Figures 16 to 22 It is according to various aspects of this application that the workpiece is displayed according to Fig.15 A partial cross-sectional view of an embodiment of the method during manufacture is shown. DETAILED DESCRIPTION
[0069] The following disclosure provides many different embodiments or examples for realizing different features of the present invention. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are only examples and are not intended to be limiting. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly contacted, and may also include an embodiment in which an additional component may be formed between the first component and the second component, so that the first component and the second component may not be in direct contact. In addition, the application may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the individual embodiments and / or configurations discussed.
[0070] In addition, forming a component on another component, forming a component connected to another component, and / or forming a component coupled to another component in the subsequent present application may include embodiments in which the components are formed in direct contact, and may also include embodiments in which additional components can be formed between the first component and the second component, so that the components may not be in direct contact. In addition, in order to facilitate the description of the relationship between one component and another component in the present invention, spatially relative terms are used, such as "lower", "upper", "horizontal", "vertical", "above", "above", "below", "below", "upward", "downward", "top", "bottom", etc. and their derivatives (for example, "horizontally", "downwardly", "upwardly", etc.). Spatially relative terms are intended to cover different orientations of devices including components.
[0071] In addition, when "about," "approximately," or the like is used to describe a numerical value or a range of numerical values, the term is intended to encompass numerical values within a reasonable range, taking into account variations that inherently occur during manufacturing as understood by those of ordinary skill in the art. For example, based on known manufacturing tolerances associated with manufacturing components having characteristics associated with the numerical value, the numerical value or range of numerical values encompasses a reasonable range including the described numerical value, such as within + / - 15% of the described numerical value. For example, a material layer having a thickness of "about 5 nanometers" may encompass a size range from 4.25 nanometers to 5.75 nanometers, where the manufacturing tolerances associated with the deposited material layer are known to those of ordinary skill in the art as + / - 15%. Further, the present application may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity and does not in itself indicate a relationship between the individual embodiments and / or configurations discussed.
[0072] Deep trench isolation (DTI) structures, such as BDTI (backside DTI) structures and FDTI (frontside DTI or full-depth DTI) structures, have been selected as a promising inter-pixel isolation method for CMOS image sensors. Generally, the DTI structure defines a unit cell with a unit size. Each unit cell provides a pixel area to accommodate the elements of one pixel. However, with the aggressive pace of scaling down, the optical crosstalk between two adjacent pixels becomes more and more serious.
[0073] The present application generally relates to image sensors, and more specifically to complementary metal oxide semiconductor (CMOS) image sensors with deep trench isolation (DTI) structures, which define an array of pixel areas for allowing components of pixels to reside therein. In some embodiments, the DTI structure is a hybrid structure extending through a substrate and includes an upper portion and a lower portion, which includes a first layer sandwiched by a second layer. The first layer is separated from the substrate by the second layer. The refractive index of the first layer can be less than the refractive index of the second layer, so that at least a portion of the incident light can be reflected to the corresponding pixel. The second layer can be a conductive layer, and a bias voltage can be applied to the DTI structure through the conductive layer to cause carrier accumulation and thereby reduce dark current. In some embodiments, the second layer is separated from the substrate by a dielectric layer. By forming the above-mentioned hybrid DTI structure, electrical isolation and optical isolation of adjacent pixels can be achieved, quantum efficiency can be increased, and optical crosstalk can be reduced.
[0074] Various aspects of the present application will now be described in more detail with reference to the accompanying drawings. In this regard, Figure 1 1 is a flow chart of a method 100 for forming a semiconductor device having a front side deep trench isolation (FDTI) structure according to an embodiment of the present application. The method 100 is combined with Figures 2 to 14 Give a description. Figures 2 to 14 are partial cross-sectional views of a workpiece 200 at different manufacturing stages according to an embodiment of the method 100 . Fig.15 The present invention includes a flowchart illustrating another method 300 for forming a semiconductor device having a backside deep trench isolation (BDTI) structure according to an embodiment of the present application. The method 300 is described below in conjunction with Figures 16 to 22 Give a description. Figures 16 to 22 is a partial cross-sectional view of a workpiece 400 at different manufacturing stages according to an embodiment of method 300. Methods 100 and 300 are merely examples and are not intended to limit the contents of the present application to those explicitly shown therein. Additional steps may be provided before, during, and after method 100 and / or method 300, and some of the steps described may be replaced, removed, or moved for other embodiments of the method. For simplicity, not all steps are described in detail herein. Since workpiece 200 / 400 will be manufactured into semiconductor device 200 / 400 or image sensor 200 / 400 at the end of this manufacturing process, workpiece 200 / 400 may be referred to as semiconductor device 200 / 400 or image sensor 200 / 400 as the context requires. Methods 100 and 300 may be used to form deep trench isolation structures in stacked silicon CMOS image sensors, non-stacked image sensors, and other suitable structures. For the avoidance of doubt, the X, Y, and Z directions in the figure are perpendicular to each other, and each Figure 1Throughout this application, unless otherwise stated, like reference numerals refer to like features.
[0075] Reference Figure 1 and Figure 2 , the method 100 includes a step 102 of receiving a workpiece 200. The workpiece 200 includes a first substrate 202. In one embodiment, the first substrate 202 is a mass-produced silicon substrate (i.e., includes mass-produced single crystal silicon). In various embodiments, the first substrate 202 may include other semiconductor materials, such as germanium, silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, indium antimonide, SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, GaInAsP, or combinations thereof. In some alternative embodiments, the first substrate 202 may be a semiconductor-on-insulator substrate, such as a silicon-on-insulator (SOI) substrate, a silicon-germanium-on-insulator (SGOI) substrate, or a germanium-on-insulator (GOI) substrate, and includes a carrier, an insulator located on the carrier, and a semiconductor layer located on the insulator. The first substrate 202 includes a first surface 202a and a second surface 202b opposite to each other. Figure 2 In the illustrated embodiment, the first surface 202a is the top surface or front-side surface of the first substrate 202, and the second surface 202b is the bottom surface or back-side surface of the first substrate 202. The workpiece 200 includes a plurality of pixel regions 1000 for forming pixels and a plurality of isolation regions 2000 for forming isolation structures. After the manufacturing process in the method 100 is completed, the isolation structures (e.g., Fig.13 The isolation structure 240 shown in FIG. 2 will isolate adjacent pixel regions 1000. The isolation region 2000 may be disposed at the edge of each pixel region 1000, so that each pixel region 1000 may be defined as an isolation structure to be formed when viewed from above (eg, Fig.13 A closed space surrounded by the walls of the isolation structure 240 shown in FIG.
[0076] The workpiece 200 includes a plurality of first isolation structures 204 formed in the front side of the isolation region 2000. Figure 2, the workpiece 200 also includes one or more second isolation structures 206 formed in each pixel region 1000 to isolate adjacent components (e.g., transistors and photodiodes) in the same pixel region 1000. It should be noted that in an embodiment in which the pixel includes a continuous active area, the workpiece 200 may not include the second isolation structure 206 in the pixel region 1000. The first isolation structure 204 and the second isolation structure 206 may also be referred to as a first shallow trench isolation (STI) structure 204 and a second STI structure 206, respectively. In some embodiments, the first STI structure 204 and the second STI structure 206 may include silicon oxide, silicon oxynitride, fluorine-doped silicate glass (FSG), a low-k dielectric material, a combination thereof, and / or other suitable materials. The first STI structure 204 and the second STI structure 206 may be formed simultaneously or sequentially in any order.
[0077] In one embodiment, the formation of the first STI structure 204 and the second STI structure 206 includes: forming a protection layer 203 on the first surface 202a of the first substrate 202; performing a patterning process on the protection layer 203 to form a plurality of openings exposing a portion of the first substrate 202; removing the portion of the first substrate 202 exposed by the opening to form a plurality of trenches; forming one or more dielectric layers above the first substrate 202 to fill the trenches, and performing a planarization process (e.g., a chemical mechanical polishing (CMP) process) to remove excess material on the protection layer 203 to form the first STI structure 204 and the second STI structure 206. In some embodiments, the planarization process may be stopped when reaching the top surface of the protection layer 203, and the protection layer 203 is used to protect the first substrate 202 during the planarization process. The patterning process applied to the protective layer 203 may include multiple processes, for example, may include: forming a photoresist layer (not shown) over the protective layer 203, and exposing the photoresist layer to a radiation source using a photomask, then developing the photoresist layer to form a patterned photoresist layer, and then etching the protective layer 203 using the patterned photoresist layer as an etching mask to form a plurality of openings. The protective layer 203 may include silicon nitride, silicon carbonitride, silicon oxycarbide, silicon oxynitride, silicon oxycarbonitride, other suitable materials, or combinations thereof, and may be formed by chemical vapor deposition (CVD), physical vapor deposition (PVD), other suitable methods, or combinations thereof.
[0078] refer to Figure 1 , Figure 3 and Figure 4 The method 100 includes a step 104 of removing a portion of the first STI structure 204 and a portion of the first substrate 202 directly below the first STI structure 204 to form a first trench 212. Figure 3As shown, the formation of the first trench 212 includes forming a patterned hard mask layer 208 over the workpiece 200. The patterned hard mask layer 208 includes an opening 210 that exposes a portion of the first STI structure 204. Figure 3 In the illustrated embodiment, the width of the opening 210 along the X direction is less than the width of the first STI structure 204. In some other embodiments, instead of using the patterned hard mask layer 208, other suitable masking films may be used to facilitate the formation of the first trench 212. Referring now to Figure 4 , using the patterned hard mask layer 208 as an etching mask, an etching process is performed to vertically extend the opening 210 downward to form a first trench 212. More specifically, the etching process removes a portion of the first STI structure 204 exposed by the opening 210 and a portion of the first substrate 202 directly below the portion of the first STI structure 204 to form the first trench 212. Figure 4 In the illustrated embodiment, the first trench 212 extends through the first STI structure 204. In addition, the first trench 212 extends substantially through the first substrate 202 but does not reach the second surface 202b of the first substrate 202. The first trench 212 may be as shown in FIG. Figure 4 The tapered trench shown in FIG. 2 may be a trench with substantially vertical sidewalls. The etching process may be a dry etching process using a suitable etchant, a wet etching process, or a combination thereof. In one embodiment, after forming the first trench 212, the patterned hard mask layer 208 is selectively removed. In another embodiment, instead of removing the patterned hard mask layer 208 immediately after forming the first trench 212, the patterned hard mask layer 208 may be removed by a subsequent etching process 224 ( Fig. 9 ) remove the patterned hard mask layer 208.
[0079] refer to Figure 1 and Figure 5 ( Figure 51 and 1 ), the method 100 includes a step 106 of forming a doped region 214 along the sidewalls and bottom surface of the first trench 212. A plasma doping process (e.g., plasma immersion ion implantation) may be performed to form the doped region 214. The plasma doping process implants one or more ion species into a portion of the first substrate 202 through the sidewalls and bottom surface of the first trench 212. The doping polarity of the doped region 214 is the same as the doping polarity of the first substrate 202, that is, the doping polarity of the doped region 214 is opposite to the doping polarity of the photosensitive element to be formed in the first substrate 202, and the doping concentration of the doped region 214 is higher than the doping concentration of the first substrate 202. In an embodiment where the first substrate 202 is a p-type substrate, the photosensitive element (not shown) to be formed includes an n-type region formed in the p-type substrate 202, and the doped region 214 is a p-type doped region (e.g., doped with boron), so that holes will accumulate at the sidewalls of the first trench 212, thereby isolating dangling bonds and / or defects at the interface between the first substrate 202 and the first trench 212 to reduce dark current and white pixels. In an embodiment where the first substrate 202 is an n-type substrate and the photosensitive element (not shown) to be formed includes a p-type region formed in the n-type substrate 202, the doped region 214 is an n-type doped region 214, the plasma implanted species may include, for example, phosphorus, and electrons will accumulate at the sidewalls of the first trench 212.
[0080] refer to Figure 1 and Figure 6 , the method 100 includes a step 108 of forming a dielectric liner 216 in the first trench 212 to electrically isolate the conductive layer 218 to be formed from the first substrate 202. In some embodiments, the dielectric liner 216 may include silicon oxide, silicon nitride, silicon carbon nitride oxide, silicon carbon nitride, silicon nitride oxide, other suitable materials, or combinations thereof. The dielectric liner 216 may be formed using a suitable method, such as atomic layer deposition (ALD), chemical vapor deposition (CVD), thermal oxidation, or other suitable methods. Figure 6 In the illustrated embodiment, the dielectric liner 216 is formed by thermal oxidation and is thus formed only on the surface of the first substrate 202 exposed by the first trench 212. That is, the dielectric liner 216 does not extend along the sidewall surface of the first STI structure 204 exposed by the first trench 212. In embodiments where the first substrate 202 includes silicon, the dielectric liner 216 includes silicon oxide. The dielectric liner 216 partially fills the first trench 212. In embodiments where the dielectric liner 216 is formed by a deposition process, the dielectric liner 216 may be formed on the workpiece 200, including on the sidewalls and bottom surface of the first trench 212, and on the top surfaces of the first STI structure 204, the second STI structure 206, and the protective layer 203.
[0081] refer to Figure 1 and Figure 7 , the method 100 includes a step 110 of conformally forming a conductive layer 218 above the workpiece 200, wherein conformally forming the conductive layer 218 above the workpiece 200 includes: conformally forming the conductive layer 218 above the protective layer 203, the second STI structure 206 and the top surface of the first STI structure 204 and the sidewalls of the first STI structure 204 and the dielectric liner 216 to partially fill the first trench 212. For the convenience of describing the layer having a substantially uniform thickness above various regions in this application, the term "conformally" may be used. In some embodiments, the conductive layer 218 may include doped polysilicon, titanium nitride, aluminum, tungsten, other suitable materials, or combinations thereof, and may be deposited using processes such as CVD, ALD, or other suitable processes. In one embodiment, the conductive layer 218 includes doped polysilicon, and the doping polarity of the conductive layer 218 is the same as the doping polarity of the doped region 214. For example, when the first substrate 202 is a p-type substrate and the doped region 214 is a p-type region, the conductive layer 218 may be p-type doped polysilicon. Polysilicon may absorb incident light, resulting in reduced quantum efficiency. In embodiments where the pixel and DTI structure have small sizes to achieve the required density, the deposition thickness of polysilicon will be so small that the incident light may penetrate the polysilicon and enter the adjacent pixel, resulting in optical crosstalk. In order to improve the optical performance of the DTI structure while ensuring the electrical performance provided by the conductive layer 218, the conductive layer 218 is intentionally formed to partially fill the first trench 212, and the filling layer 220 (see FIG. 2 ) to be formed is formed. Figure 8 ) will be used to reflect light back to the corresponding pixel.
[0082] refer to Figure 1 and Figure 8 , the method 100 includes a step 112 of forming a filling layer 220 above the workpiece 200 to substantially fill the first trench 212. In the present embodiment, the filling layer 220 is configured to have a different composition than the conductive layer 218. The refractive index of the filling layer 220 is less than the refractive index of the conductive layer 218, so that the incident light can be substantially or completely reflected back to the pixel to be subsequently formed in the pixel area 1000, thereby increasing the quantum efficiency and advantageously reducing or substantially eliminating the optical crosstalk between adjacent pixels. Therefore, the signal-to-noise ratio can be improved and the image integrity can be improved. In some embodiments, the filling layer 220 may include silicon oxide, silicon nitride, silicon carbide, a combination thereof, or other suitable materials, and may be formed by any suitable method, including CVD, ALD, other methods, or a combination thereof. In one embodiment, the conductive layer 218 includes doped polysilicon, and the filling layer 220 includes silicon oxide. In some embodiments, as Figure 8As shown, the workpiece 200 may include a gap (or air gap or void) 217 sealed or surrounded by a filling layer 220. In some embodiments, the filling layer 220 may be a multi-layer structure. For example, the deposition of the filling layer 220 may include conformally depositing a first filling layer over the conductive layer 218 and conformally depositing a second filling layer over the first filling layer. The composition of the second filling layer is different from the composition of the first filling layer, for example, to increase the reflectivity of the composite DTI structure 228 to be formed.
[0083] refer to Figure 1 and Fig. 9 , the method 100 includes a step 114 of etching back the conductive layer 218 and the filling layer 220 by an etching process 224. In one embodiment, the etching process 224 selectively etches the portion of the conductive layer 218 and the filling layer 220 located above the first surface 202a and the portion of the conductive layer 218 and the filling layer 220 located in the upper portion of the first trench 212 to form a second trench 226 without substantially etching the protective layer 203. In an embodiment in which the dielectric liner 216 is formed by a deposition process, the etching process 224 may also recess the dielectric liner 216. The etching process 224 may be a dry etching process, a wet etching process, or a combination thereof using a suitable etchant. The recessed conductive layer 218, the recessed filling layer 220, the (recessed) dielectric liner 216, and the doped region 214 may be collectively referred to as a deep trench isolation (DTI) structure 228, and the DTI structure 228 is formed in the lower portion of the first trench 212. In some embodiments, DTI structure 228 may include gap 217. Fig. 9 In the illustrated embodiment, the conductive layer 218 is spaced apart from the first substrate 202 by the dielectric liner 216, and the filling layer 220 is spaced apart from the dielectric liner 216 by the conductive layer 218. In other words, the filling layer 220 is embedded in the conductive layer 218, the conductive layer 218 is embedded in the dielectric liner 216, and the top surface of the DTI structure 228 includes the top surface of the conductive layer 218 and the top surface of the filling layer 220. The depth of the second trench 226 can be controlled by the duration of the etching process 224. Fig. 9 In the illustrated embodiment, the depth of the second trench 226 is substantially equal to the depth of the first STI structure 204 to prevent or reduce any current leakage from the front side of the workpiece 200. That is, the bottom surface of the first STI structure 204 can be substantially coplanar with the top surface of the DTI structure 228. In embodiments where there is a low etch selectivity between the first STI structure 204 and the second STI structure 206 and the filling layer 220, the first STI structure 204 and the second STI structure 206 can be slightly etched by the etching process 224.
[0084] refer to Figure 1 and Fig.10 , the method 100 includes a step 116 of depositing a dielectric layer 230 over the workpiece 200 to refill the second trench 226. The dielectric layer 230 may be referred to as a refill layer 230. The dielectric layer 230 is deposited over the workpiece 200 and in the second trench 226 using a suitable method (e.g., ALD, CVD, or other suitable method). The dielectric layer 230 may include silicon oxide, silicon nitride, silicon oxycarbide, silicon oxycarbonitride, silicon carbonitride, metal nitride, or a suitable dielectric material. In some embodiments, the composition of the dielectric layer 230 may be the same as the composition of the first STI structure 204. For example, the first STI structure 204 and the dielectric layer 230 may both include silicon oxide. In some embodiments, the composition of the dielectric layer 230 may be different from the composition of the first STI structure 204. For example, the first STI structure 204 may include silicon oxide, and the dielectric layer 230 may include silicon nitride.
[0085] Still refer to Figure 1 and Fig.10 , the method 100 includes a step 118 of performing a planarization process to remove excess dielectric material of the dielectric layer 230 above the protection layer 203 and leaving the dielectric layer 230 in the second trench 226. The planarization process may include a CMP process, and the CMP process may be stopped when the CMP process reaches the top surface of the protection layer 203. The conductive layer 218 in the DTI structure 228 is thus covered by the dielectric layer 230 to reduce current leakage. In the embodiment where the first STI structure 204 and the second STI structure 206 are slightly etched back by the etching process 224, as shown in FIG. Fig.10 As shown, dielectric layer 230 is also formed on recessed first STI structure 204 and recessed second STI structure 206. First STI structure 204 and dielectric layer 230 formed in second trench 226 may be collectively referred to as first STI structure 204'.
[0086] refer to Fig.11 , the protective layer 203 can be selectively removed (e.g., using an etchant including phosphoric acid) to expose the first surface 202a of the first substrate 202. In some embodiments, after forming the DTI structure 228, components such as a photodiode 231 and a plurality of transistors (e.g., a transfer transistor, a reset transistor, a source follower) can be formed to form a pixel (not explicitly shown) in each pixel region 1000. In some other embodiments, each pixel may include a photodiode 231, and two or more pixels may share one or more of the plurality of transistors. Each transistor in the pixel may include a gate structure (e.g., a gate electrode) formed above the first surface 202a of the first substrate 202 in the pixel region 1000. Fig.11Although not explicitly shown, the gate structure 233 may include a gate dielectric layer and a gate electrode layer located above the gate dielectric layer. It should be understood that the photodiode 231 is used for illustration purposes only and is not intended to limit the present disclosure to that explicitly described therein.
[0087] refer to Fig.12 , after forming the photodiode 231 and transistor of the pixel in the pixel area 1000, a first interconnect structure 232 is formed over the first surface 202a of the substrate 202. In some embodiments, the first interconnect structure 232 may include a plurality of interlayer dielectric (ILD) layers and a plurality of metal lines or contact vias in each ILD layer. The metal lines and contact vias in each ILD layer may be formed of a metal (e.g., aluminum, tungsten, ruthenium, or copper). Because the first interconnect structure 232 is formed over the front side of the workpiece 200, the first interconnect structure 232 may also be referred to as a front side interconnect structure 232. In an embodiment where the first substrate 202 is a p-type substrate, a negative voltage may be applied to the conductive layer 218 to cause hole accumulation at the sidewalls of the DTI structure 228 and isolate dangling bonds and / or defects at the interface between the first substrate 202 and the DTI structure 228, thereby reducing dark current and white pixels. A negative voltage may be applied to the conductive layer 218 through the metal lines and contact vias in the first interconnect structure 232. In embodiments where first substrate 202 is an n-type substrate, a positive voltage may be applied to conductive layer 218 to induce electron accumulation at the sidewalls of DTI structure 228 .
[0088] Reference Fig.13 After forming the first interconnect structure 232, the second substrate 234 is bonded or attached to the first interconnect structure 232. In some embodiments, the second substrate 234 can be bonded to the workpiece 200 by fusion bonding, using an adhesive layer, or a combination thereof. In some examples, the second substrate 234 can be a carrier substrate and can include a semiconductor material (e.g., silicon), sapphire, glass, a polymer material, or other suitable material. In some embodiments, the second substrate 234 can include an application specific integrated circuit (ASIC).
[0089] Reference Figure 1 and Fig.13 , the method 100 includes a step 120 of turning the workpiece 200 over, such as Fig.13As shown, the first substrate 202 is on top and disposed above the first interconnect structure 232. Then, the workpiece 200 is thinned, planarized, recessed, or ground from the second surface 202b until the filling layer 220 in the DTI structure 228 is exposed. The combination of the DTI structure 228 and the first STI structure 204′ (including the first STI structure 204 and the filling layer 230) completely extends through the first substrate 202 and can be collectively referred to as a DTI structure 240. Therefore, the pixels formed in the pixel region 1000 are electrically and optically isolated from the pixels in the adjacent pixel region 1000 by the DTI structure 240.
[0090] refer to Figure 1 and Fig.14 , the method 100 includes a step 122 of performing further processes. Such further processes may include forming a color filter 244 covering the photodiode of the workpiece 200 over the second surface 202b, and forming a microlens 248 over the color filter 244. Other suitable processes may be further performed to complete the manufacture of the semiconductor device 200, and in one embodiment, the semiconductor device 200 is a back-illuminated image sensor.
[0091] In the above reference Figures 1 to 14 In the depicted embodiment, the DTI structure 228 is formed from the front side (eg, the first surface 202a) of the first substrate 202. Figures 15 to 22 In the depicted embodiment, the DIT structure is formed from the back side (eg, the second surface 202b) of the first substrate 202. Unless otherwise noted, like reference numerals denote like features, and repeated descriptions are omitted for simplicity.
[0092] Reference now Fig.15 and Fig.16 , the method 300 includes a step 302 of receiving a workpiece 400. The workpiece 400 includes a first substrate 202 having a pixel region 1000 and an isolation region 2000. As described above with reference Figure 2 As described above, each isolation region 2000 is disposed between two adjacent pixel regions 1000. The workpiece 400 further includes a plurality of pixels. Each pixel is formed in a corresponding pixel region 1000 and may include the same Fig.11 The photodiode 231 depicted is similar to the photodiode 405 and one or more transistors having a gate structure 233. Note that, Fig.16The photodiode 405 shown in is for illustrative purposes only and is not intended to limit the present disclosure to the contents explicitly described therein. The workpiece 400 also includes a plurality of first STI structures 204, and each first STI structure 204 is formed in a corresponding isolation region 2000. The first STI structure 204 includes a bottom surface 204b. The workpiece 400 also includes a plurality of second STI structures 206, and each second STI structure 206 is formed in a corresponding pixel region 1000 to isolate adjacent components (e.g., transistors) in the pixel region 1000. The number of second STI structures 206 in the pixel region 1000 is only an example and is not intended to be limiting. For example, in some embodiments, some pixels in the workpiece 400 may not include a second STI structure 206. The workpiece 400 also includes a first interconnect structure 232 formed above the first surface 202a of the first substrate 202.
[0093] Reference Fig.15 and Fig.17 The method 300 includes a step 304 of flipping the workpiece 400 over and thinning it to a predetermined thickness to form a satisfactory backside trench isolation structure. Fig.17 In the embodiment shown in , after forming the first interconnect structure 232, the second substrate 234 is bonded or attached to the first interconnect structure 232, and then the workpiece 400 is turned over and the workpiece 200 is planarized, recessed or ground from the second surface 202b. Then, as shown in Fig.17 As shown, a pattern film 410 is formed on the second surface 202b of the first substrate 202, and the pattern film 410 is patterned to form a plurality of openings exposing a portion of the first substrate 202. The pattern film 410 may be a hard mask layer similar to the hard mask layer 208, or may be a photoresist layer.
[0094] Reference Fig.15 and Fig.17 , the method 300 includes performing an etching process to etch the back side of the first substrate 202 to form a third trench 415 exposing the first STI structure 204. The etching process is performed using the patterned pattern film 410 as an etching mask to form a plurality of third trenches 415 extending from the second surface 202b of the first substrate 202 to the first STI structure 204. That is, the third trenches 415 expose a portion of the first STI structure 204. Fig.17In the embodiment shown in , the third trench 415 exposes a portion of the bottom surface 204b of the first STI structure 204. In some other embodiments, the third trench 415 may also expose the sidewall surface of the first STI structure 204. The etching process may be a dry etching process, a wet etching process, or a combination thereof using a suitable etchant. It should be noted that, because the photodiode 405 and the transistor of the pixel have been formed in the pixel area 1000, in order to ensure the reliability of the components of the pixel (such as the photodiode 405 and the transistor, etc.), a high temperature process (such as annealing) is not performed to activate the dopant to ion-dope the third trench 415.
[0095] refer to Fig.15 and Fig.18 , the method 300 includes a step 308 of forming a first dielectric liner 420 on the sidewalls and bottom surface of the third trench 415 and over the workpiece 400. In one embodiment, the first dielectric liner 420 is conformally deposited so that it has a substantially uniform thickness above the top surface of the workpiece 400 and partially fills the third trench 415. Because the components of the pixel (such as the photodiode 405 and the transistor, etc.) have been formed in the pixel area 1000, the first dielectric liner 420 is formed at a low temperature so that the formation of the first dielectric liner 420 does not significantly damage the components in the pixel area 1000. For example, the first dielectric liner 420 is formed below 400°C. In some embodiments, the first dielectric liner 420 can be formed by a plasma oxidation process, a CVD process, or other suitable processes. The first dielectric liner 420 can be formed of silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride, silicon oxynitride, TEOS, doped silicon oxide (e.g., BPSG, FSG, PSG, BSG, etc.) or other suitable materials. In one embodiment, the first dielectric liner 420 is formed of a low-k dielectric layer.
[0096] Still refer to Fig.15 and Fig.18 The method 300 includes a step 310 of conformally forming a second dielectric liner 425 above the first dielectric liner 420 and in the third trench 415. The second dielectric liner 425 may be formed by performing a deposition process such as a CVD process, an ALD process, or other suitable deposition process. The second dielectric liner 425 may include a high-k (dielectric constant greater than the dielectric constant of silicon oxide, about 3.9) dielectric material, such as hafnium oxide, titanium oxide (TiO2), hafnium zirconium oxide (HfZrO), tantalum oxide (Ta 2 O 5 ), Hafnium Silicon Oxide (HfSiO 4 ), zirconium oxide, zirconium oxide (ZrSiO 2 ), lanthanum oxide (La 2 O3 ), aluminum oxide (Al 2 O 3 ), yttrium oxide (Y 2 O 3 )、SrTiO 3 (STO), BaTiO 3 (BTO), BaZrO, Hafnium Lanthanum Oxide (HfLaO), Lanthanum Silicon Oxide (LaSiO), Aluminum Silicon Oxide (AlSiO), Hafnium Tantalum Oxide (HfTaO), Hafnium Titanium Oxide (HfTiO), (Ba, Sr)TiO 3 (BST), silicon nitride (SiN), silicon oxynitride (SiON), combinations thereof, or other suitable materials. Forming the high-k second dielectric liner 425 can enhance carrier accumulation at the sidewalls of the third trench 415, thereby reducing dark current and white pixels. It is worth noting that the second dielectric liner 425 is optional, and in some embodiments, the related operations for forming the second dielectric liner 425 (i.e., Fig.15 310 of step 310).
[0097] refer to Fig.15 and Fig.19 , the method 300 includes a step 312 of conformally forming a conductive layer 430 above the second dielectric liner 425 and in the third trench 415. The first dielectric liner 420 and the second dielectric liner 425 separate the conductive layer 430 from the first substrate 202. The first dielectric liner 420 and the second dielectric liner 425 also separate the conductive layer 430 from the first STI structure 204. Figure 7 Unlike the described embodiments, after forming the photodiode 405 and transistor of the pixel, a conductive layer 430 that does not include doped polysilicon is formed, so there is no need to perform a high temperature process (e.g., an annealing process) to activate the dopant in the doped polysilicon. In some embodiments, the conductive layer 430 may include titanium nitride (TiN), tantalum nitride (TaN), aluminum (Al), tungsten (W), nickel (Ni), titanium (Ti), ruthenium (Ru), cobalt (Co), platinum (Pt), copper (Cu), or other suitable metal materials or combinations thereof. In various embodiments, the conductive layer 430 may be formed by ALD, PVD, CVD, or other suitable processes. In some embodiments, a bias voltage may be applied to the conductive layer 430 to cause carrier accumulation, thereby reducing dark current.
[0098] refer to Fig.15 , Fig. 20 and Fig.21, the method 300 includes a step 314 of depositing a filling layer 435 over the workpiece 400 to substantially fill the third trench 415. In some embodiments, the conductive layer 430 may absorb a portion of the incident light and / or reflect only a portion of the incident light to the corresponding pixel. The refractive index of the filling layer 435 may be less than the refractive index of the conductive layer 430, so that the filling layer 435 may reflect most of the incident light to the corresponding pixel. Thus, quantum efficiency may be increased, and optical crosstalk between adjacent pixels may be advantageously reduced or substantially eliminated. The filling layer 435 may include silicon oxide, silicon nitride, silicon carbide, combinations thereof, or other suitable materials, and may be formed by any suitable method, including CVD, ALD, other methods, or combinations thereof. The first dielectric liner 420, the second dielectric liner 425, the conductive layer 430, and the filling layer 435 may be collectively referred to as an isolation structure 440. In some embodiments, the workpiece 400 may include a gap (or air gap or void) 437 sealed or surrounded by the filling layer 435, for example Fig. 20 As shown in the isolation structure 440 on the right side of FIG.
[0099] refer to Fig.21 After forming the isolation structure 440, a planarization process may be performed to remove excess material and complete the final structure of the isolation structure 440. For example, the planarization process may remove the patterned pattern film 410 and the material located above the patterned pattern film 410. The combination of the isolation structure 440 and the first STI structure 204 completely extends through the first substrate 202. Therefore, adjacent pixels formed in the adjacent pixel region 1000 may be electrically and optically isolated from each other by the combination of the isolation structure 440 and the first STI structure 204.
[0100] refer to Fig.15 and Fig. 22 , the method 300 includes a block step 316 of performing further processes. The further processes may include forming a color filter 445 covering the photodiode of the workpiece 400 over the second surface 202b. The further processes may include forming a microlens 450 over the color filter 445. Other suitable processes may be further performed to complete the fabrication of the semiconductor device 400.
[0101] Although not intended to be limiting, one or more embodiments of the present application provide many benefits to image sensors and imaging systems. For example, by forming a hybrid DTI structure, a pixel can be electrically and optically isolated from its neighboring pixels. Optical crosstalk can be advantageously reduced or even substantially eliminated, and quantum efficiency can be advantageously increased. In addition, the disclosed method can be easily integrated into existing semiconductor manufacturing processes.
[0102] The present application provides many different embodiments. The present application discloses semiconductor structures and methods for manufacturing the same. In one exemplary aspect, the present application relates to a method for forming an image sensor. The method includes receiving a workpiece including a first isolation structure, the first isolation structure being formed in the front side of a substrate; forming a trench extending through the first isolation structure and a portion of the substrate; forming a dielectric liner to line the trench; after forming the dielectric liner, conformally depositing a conductive layer above the workpiece; and depositing a fill layer above the conductive layer to fill the trench.
[0103] In some embodiments, the refractive index of the conductive layer is greater than the refractive index of the filling layer. In some embodiments, the conductive layer includes doped polysilicon, titanium nitride, aluminum, or tungsten. In some embodiments, the filling layer includes silicon oxide, silicon nitride, or silicon carbide. In some embodiments, the method may further include: forming an interconnect structure above the front side of the substrate, the interconnect structure including an interlayer dielectric layer and a conductive component located in the interlayer dielectric layer, wherein the conductive component is electrically coupled to the conductive layer; and, applying a bias voltage to the conductive layer via the conductive component. In some embodiments, depositing the filling layer includes: conformally depositing a first filling layer above the conductive layer; and, conformally depositing a second filling layer above the first filling layer, wherein the composition of the second filling layer is different from the composition of the first filling layer. In some embodiments, the method may further include: etching back the conductive layer and the filling layer to form a second trench in the trench; depositing a dielectric layer on the workpiece to fill the second trench; and, performing a planarization process on the workpiece. In some embodiments, the workpiece also includes a protective layer formed above the front side of the substrate, wherein the top surface of the protective layer is coplanar with the top surface of the first isolation structure; and, wherein performing the planarization process includes: removing excess material on the protective layer. In some embodiments, the method may further include: after depositing the dielectric filling layer, flipping the workpiece; and, performing a planarization process on the back side of the substrate to expose the filling layer, the back side of the substrate being opposite to the front side of the substrate. In some embodiments, the method may further include: before performing the planarization process on the back side of the substrate, forming a first photosensitive element and a second photosensitive element in the substrate, wherein the first photosensitive element and the second photosensitive element are isolated by a dielectric liner, a conductive layer and a filling layer. In some embodiments, forming the dielectric liner includes: thermally oxidizing the workpiece; wherein, after depositing the conductive layer, a first portion of the conductive layer is in direct contact with the dielectric liner, and a second portion of the conductive layer is in direct contact with the first isolation structure. In some embodiments, forming the dielectric liner includes: performing a deposition process on the workpiece; wherein the conductive layer is separated from the first isolation structure by the dielectric liner. In some embodiments, forming a groove includes: forming a patterned hard mask layer above the workpiece, the patterned hard mask layer including an opening exposing a portion of the first isolation structure; and performing an etching process using the patterned hard mask layer as an etching mask to remove a portion of the first isolation structure and a portion of the substrate, wherein a portion of the substrate is located directly below the portion of the first isolation structure.
[0104] In another exemplary aspect, the present disclosure relates to a method for forming an image sensor. The method includes receiving a workpiece including a first isolation structure formed in a front side of a substrate; forming a trench extending through the first isolation structure and a portion of the substrate; forming a doped region along a sidewall and a bottom surface of the trench, the doped region including a dopant having the same doping polarity as the substrate; after forming the doped region, forming a dielectric liner to line the trench; after forming the dielectric liner, conformally depositing a conductive layer over the workpiece; and depositing a filling layer over the conductive layer to fill the trench.
[0105] In yet another exemplary aspect, the present disclosure relates to a semiconductor device. The semiconductor device includes: a substrate having a front-side surface and a back-side surface; a first photosensitive element and a second photosensitive element disposed in the substrate; and an isolation structure extending through the substrate and disposed between the first photosensitive element and the second photosensitive element; wherein the isolation structure includes an upper portion and a lower portion located directly below the upper portion, wherein the upper portion is closer to the front-side surface than the lower portion, and wherein the lower portion includes: a first dielectric layer extending from the upper portion to the back-side surface; a conductive layer surrounding a sidewall surface of the first dielectric layer; and a second dielectric layer surrounding a sidewall surface of the conductive layer, wherein the first dielectric layer and the second dielectric layer are separated by the conductive layer.
[0106] In some embodiments, the conductive layer is biased to a predetermined voltage. In some embodiments, the refractive index of the conductive layer is greater than the refractive index of the first dielectric layer. In some embodiments, the semiconductor device may further include: a first color filter disposed below the first photosensitive element; and, a second color filter disposed below the second photosensitive element. In some embodiments, the conductive layer includes doped polysilicon, and the first dielectric layer includes silicon oxide. In some embodiments, the lower portion further includes: a doped region surrounding a sidewall surface of the second dielectric layer; wherein the doped region includes a dopant having a first doping polarity, and the first photosensitive element and the second photosensitive element include another doped region having a second polarity opposite to the first doping polarity.
[0107] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present application as a substrate to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that this equivalent configuration does not deviate from the spirit and scope of the present invention, and in the case of not deviating from the spirit and scope of the present invention, they can make multiple changes, replacements and changes herein.
Claims
1. A method for forming an image sensor, characterized in that: include: receiving a workpiece including a first isolation structure formed in a front side of a substrate; forming a first trench extending through the first isolation structure and a portion of the substrate; forming a dielectric liner to line the first trench; after forming the dielectric liner, conformally depositing a conductive layer over the workpiece; depositing a filling layer over the conductive layer to fill the first trench; Etching back the conductive layer and the filling layer to form a second trench in the first trench; as well as A dielectric layer is deposited over the workpiece to fill the second trench.
2. The method according to claim 1, characterized in that The refractive index of the conductive layer is greater than the refractive index of the filling layer.
3. The method according to claim 1, characterized in that The conductive layer includes doped polysilicon, titanium nitride, aluminum or tungsten.
4. The method according to claim 1, characterized in that: The filling layer includes silicon oxide, silicon nitride or silicon carbide.
5. The method according to claim 1, characterized in that Also includes: forming an interconnect structure over the front side of the substrate, the interconnect structure comprising an interlayer dielectric layer and a conductive feature in the interlayer dielectric layer, wherein the conductive feature is electrically coupled to the conductive layer; and, A bias voltage is applied to the conductive layer via the conductive member.
6. The method according to claim 1, characterized in that Depositing the filling layer comprises: conformally depositing a first fill layer over the conductive layer; and, A second fill layer is conformally deposited over the first fill layer, wherein a composition of the second fill layer is different from a composition of the first fill layer.
7. The method according to claim 1, characterized in that Also includes: After filling the second trench, a planarization process is performed on the workpiece.
8. The method according to claim 7, characterized in that The workpiece further includes a protection layer formed over the front side of the substrate, wherein a top surface of the protection layer is coplanar with a top surface of the first isolation structure; And, wherein performing the planarization process includes: removing excess material on the protection layer.
9. The method according to claim 1, characterized in that: Also includes: After depositing the fill layer, turning the workpiece over; as well as, A planarization process is performed on a back side of the substrate to expose the filling layer, the back side of the substrate being opposite to the front side of the substrate.
10. The method according to claim 9, characterized in that Also includes: Before performing a planarization process on the back side of the substrate, a first photosensitive element and a second photosensitive element are formed in the substrate, wherein the first photosensitive element is isolated from the second photosensitive element by the dielectric liner, the conductive layer, and the filling layer.
11. The method according to claim 1, characterized in that: The forming of the dielectric liner comprises: thermally oxidizing the workpiece; After the conductive layer is deposited, a first portion of the conductive layer is in direct contact with the dielectric liner, and a second portion of the conductive layer is in direct contact with the first isolation structure.
12. The method according to claim 1, characterized in that The forming of the dielectric liner comprises: performing a deposition process on the workpiece; The conductive layer and the first isolation structure are separated by the dielectric liner.
13. The method according to claim 1, characterized in that The forming of the first groove comprises: forming a patterned hard mask layer above the workpiece, the patterned hard mask layer comprising an opening exposing a portion of the first isolation structure; and, An etching process is performed using the patterned hard mask layer as an etching mask to remove a portion of the first isolation structure and a portion of the substrate, wherein the portion of the substrate is located directly below a portion of the first isolation structure.
14. A method of forming an image sensor, comprising: receiving a workpiece including a first isolation structure formed in a front side of a substrate; forming a third trench extending through a portion of the substrate and exposing a portion of the first isolation structure; forming a first dielectric liner along the sidewalls and bottom surface of the third trench, the first dielectric liner being formed of a low-k dielectric layer; forming a second dielectric liner to line the third trench, the second dielectric liner comprising a high-k dielectric material; after forming the second dielectric liner, conformally depositing a conductive layer over the workpiece; as well as, depositing a filling layer over the conductive layer to fill the third trench; A planarization process is performed to remove material located on the front side of the substrate.
15. A semiconductor device manufactured by the method for forming an image sensor according to any one of claims 1 or 14, characterized in that: include: a substrate having a front surface and a back surface; A first photosensitive element and a second photosensitive element disposed in the substrate; as well as, an isolation structure extending through the substrate and disposed between the first photosensitive element and the second photosensitive element; Wherein, the isolation structure comprises an upper portion and a lower portion located directly below the upper portion, wherein the upper portion is closer to the front surface than the lower portion, and wherein the lower portion comprises: a first dielectric layer extending from the upper portion to the backside surface; a conductive layer surrounding the sidewall surface of the first dielectric layer; and, A second dielectric layer surrounds the sidewall surface of the conductive layer, wherein the first dielectric layer and the second dielectric layer are separated by the conductive layer.
16. The semiconductor device according to claim 15, characterized in that The conductive layer is biased to a predetermined voltage.
17. The semiconductor device according to claim 15, characterized in that The refractive index of the conductive layer is greater than the refractive index of the first dielectric layer.
18. The semiconductor device according to claim 15, characterized in that Also includes: A first color filter disposed below the first photosensitive element; as well as, A second color filter is disposed below the second photosensitive element.
19. The semiconductor device according to claim 15, characterized in that The conductive layer includes doped polysilicon, and the first dielectric layer includes silicon oxide.