Carbon nanotube-polyaniline-Prussian blue composite material, preparation method thereof, and positive electrode material for potassium ion battery
By adding polyaniline and carbon nanotubes to the Prussian blue analog to form a composite material, the problem of poor conductivity of Prussian blue analog is solved, the high conductivity and cycle stability of the positive electrode material of the potassium ion battery is achieved, and the battery is improved performance.
Patent Information
- Application Number
- CN202211535173.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-30
AI Technical Summary
The Prussian blue analogues in the existing potassium ion battery positive electrode materials have low crystallinity and poor conductivity, resulting in poor structural stability and poor electrochemical activity during K+ insertion/deintercalation, and agglomeration problems after doping carbon nanotubes or graphene and The bonding strength is low, making it difficult to effectively improve conductivity.
Using carbon nanotube-polyaniline-Prussian blue analog composite material, the crystallinity and interconnection of Prussian blue analogs are improved by polyaniline as the nucleation active point, and combining carbon nanotubes to improve the conductivity and structural stability to form high conductivity potassium ion electrode material with high-speed performance.
The high conductivity and structural stability of Prussian blue analog is achieved. As a positive electrode material for potassium ion batteries, it has high rate performance and long cycle life, improving the stability and electrochemical activity during K+ insertion/deintercalation.
Smart Images

Figure CN115832287B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of potassium ion batteries, in particular to positive electrode materials for potassium ion batteries. Background Art
[0002] Potassium-ion batteries have attracted widespread attention due to their economic and efficient advantages. Compared with lithium batteries and sodium batteries, potassium batteries show unique advantages in cost and rate, such as high potassium reserves (about 500 times that of lithium) and the use of aluminum foil negative electrode collectors, which is expected to significantly reduce costs; compared with lithium and sodium, K + has the smallest Stokes radius (in PC solvent), indicating that K + Has the highest ionic conductivity and ion mobility (Li + In theory, potassium batteries can improve rate capability without sacrificing specific capacity. In addition, potassium batteries can operate at higher voltages over a wider voltage range, and the low melting point of potassium metal (only 63.4°C) can melt potassium dendrites and cut off short circuits before the battery goes into severe thermal runaway, thus achieving high energy density and high safety. Although potassium batteries have excellent theoretical performance, the technology is now in its infancy. Existing lithium battery electrode materials are not suitable for potassium batteries. Electrode materials need to be designed and developed for potassium batteries to manufacture fully functional potassium-ion batteries.
[0003] Among the cathode materials explored, Prussian blue analogs (PBA) and their derivatives have the characteristics of low cost, non-toxicity and high safety. + It also exhibits extremely competitive excellent performance: in non-aqueous systems, K + Than Na + and Li + Easier access to the PBA framework, enabling low lattice strain and fast ion diffusion kinetics; K + Better compatibility with PBA (K>Na>>Li) is beneficial to extend the cycle life; K + The low Gibbs free energy with PBA enables higher redox potentials, such as the average discharge voltage and energy density of KMnFe-PBA (3.7 V and 521 Wh / kg, respectively) are higher than those of NaMnFe-PBA (3.4 V and 476 Wh / kg) and LiMnFe-PBA (3.5 V and 479 Wh / kg).
[0004] In the prior art, Prussian blue analogs are usually prepared by chemical coprecipitation growth. However, the Prussian blue analog crystals thus produced contain a large amount of coordinated water and vacancies, and have low crystallinity, resulting in K + PBA has the disadvantages of poor structural stability during insertion / deintercalation and poor electrochemical activity. In addition, PBA has poor electrical conductivity.
[0005] In order to improve the conductivity of Prussian blue analogs, there are reports of doping carbon nanotubes or graphene in Prussian blue analogs. However, there is a problem that the doping of carbon nanotubes or graphene causes the Prussian blue analogs to agglomerate. In addition, there is a problem that the bonding strength between graphene, carbon nanotubes and Prussian blue analogs is not high, and only the conductivity of Prussian blue analogs close to graphene and carbon nanotubes is improved, while the problem of poor conductivity in the part of Prussian blue analogs that are not bonded to graphene and carbon nanotubes still exists. Summary of the invention
[0006] The inventors have conducted in-depth research on the above technical problems and found that in the carbon nanotube-polyaniline-Prussian blue analog composite material of the present application, polyaniline is added to provide nucleation active points for the co-deposition of Prussian blue analog to improve the crystallinity of Prussian blue analog, and the interconnection between Prussian blue analog crystals is improved to provide channels for electron transmission. The carbon nanotubes are further combined to improve the conductivity and structural stability of PBA, and the K is increased on the basis of maintaining the structural framework of the Prussian blue analog. + The structural stability and electrochemical activity during insertion / deinsertion are beneficial for achieving high-rate performance and cycle stability when used as a positive electrode material for potassium ion electrodes.
[0007] This application includes the following technical solutions:
[0008] The first aspect of the present application provides a nanotube-polyaniline-Prussian blue analog composite material, which contains carbon nanotubes, Prussian blue analogs attached to the surface of the carbon nanotubes, and polyaniline connecting the Prussian blue analogs to each other.
[0009] The second aspect of the present application provides a method for preparing a carbon nanotube-polyaniline-Prussian blue analog composite material, which comprises the following steps:
[0010] Preparation process of reaction solution A: dissolving soluble divalent manganese salt and potassium citrate in deionized water, then successively adding N-methylpyrrolidone and polyaniline, and dispersing them evenly to form reaction solution A;
[0011] Reaction solution B preparation process: adding methanol and carbon nanotube N,N-dimethylacetamide solution to potassium ferrocyanide aqueous solution and dispersing them evenly to form reaction solution B;
[0012] Co-deposition step: the reaction solution B is mixed with the reaction solution A and heated to perform co-deposition, thereby generating a carbon nanotube-polyaniline-Prussian blue analog composite material.
[0013] The third aspect of the present application provides a positive electrode material for a potassium ion battery, which comprises the aforementioned carbon nanotube-polyaniline-Prussian blue analogue composite material, or a carbon nanotube-polyaniline-Prussian blue analogue composite material obtained by the preparation method of the aforementioned carbon nanotube-polyaniline-Prussian blue analogue composite material.
[0014] A fourth aspect of the present application provides a potassium ion battery, which comprises the aforementioned positive electrode material for a potassium ion battery.
[0015] The fifth aspect of the present application provides the use of the aforementioned carbon nanotube-polyaniline-Prussian blue analogue composite material of the present invention or the carbon nanotube-polyaniline-Prussian blue analogue composite material obtained according to the aforementioned method for preparing the carbon nanotube-polyaniline-Prussian blue analogue composite material in the preparation of positive electrode materials for potassium ion batteries.
[0016] Beneficial effects:
[0017] The carbon nanotube-polyaniline-Prussian blue analog composite material of the present invention uses highly conductive carbon nanotubes as a support, and provides nucleation active points for carbon nanotube-Prussian blue analog co-deposition by adding polyaniline to improve the crystallinity of the Prussian blue analog, improve the interconnection between the Prussian blue analog crystals, provide channels for electron transmission, and further combine with carbon nanotubes to improve the conductivity and structural stability of PBA, thereby improving K while maintaining the structural framework of the Prussian blue analog. + The structural stability and electrochemical activity during insertion / deinsertion are beneficial for achieving high-rate performance and cycle stability when used as a positive electrode material for potassium ion electrodes. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a scanning electron microscope image of the carbon nanotube-polyaniline-Prussian blue analog composite material prepared in Example 1;
[0019] Figure 2 is a charge and discharge voltage-capacity diagram of the half-cell prepared in Example 1;
[0020] Figure 3 It is the capacity curve of the half-cell prepared in Example 1 after 100 cycles of charge and discharge at 0.2C, 0.5C, 1C, 2C, and 0.2C, respectively.
[0021] Figure 4 is a scanning electron microscope image of the carbon nanotube-Prussian blue analog composite material without polyaniline prepared in Comparative Example 1;
[0022] Figure 5 are impedance spectra of electrode 1 prepared in Example 1 and electrode 2 prepared in Comparative Example 1;
[0023] Figure 6 This is a charge and discharge voltage-capacity diagram of the half-cell prepared in Comparative Example 1. DETAILED DESCRIPTION
[0024] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. In the examples, those without specifying specific techniques or conditions are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. Those without specifying the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially. In the following examples, if not clearly stated, "%" refers to weight percentage.
[0025] [Carbon nanotube-polyaniline-Prussian blue analog composite material]
[0026] The carbon nanotube-polyaniline-Prussian blue analogue composite material of the present invention contains carbon nanotubes, Prussian blue analogues attached to the surface of the carbon nanotubes and polyaniline connecting the Prussian blue analogues to each other.
[0027] In some embodiments, the Prussian blue analogue is a sheet-like structure with a size of 20 to 200 nm, more preferably 40 to 100 nm. The thickness of the sheet-like structure of the Prussian blue analogue can be, for example, 10 to 20 nm.
[0028] In some embodiments, the carbon nanotubes may be single-walled carbon nanotubes or multi-walled carbon nanotubes, without particular limitation. From the perspective of electrical conductivity, multi-walled carbon nanotubes are preferred. The carbon nanotubes may be functionally modified carbon nanotubes, such as carboxyl-modified carbon nanotubes. The diameter of the carbon nanotubes may be, for example, 10 to 50 nm.
[0029] In some embodiments, the polyaniline is a lamellar structure with a thickness of 100 to 200 nm and a size of 500 nm to 1 μm.
[0030] The reversible capacity of the aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material can be, for example, 140-160 mAh / g at 0.2C and 90-100 mAh / g at 2C. The aforementioned reversible capacity can be obtained by the following test: a button half-cell is used, wherein the counter electrode is a potassium sheet, and the electrolyte is a 1 mol / L KPF6 EC (ethylene carbonate) / DMC (dimethyl carbonate) (EC to DMC volume ratio is 1:1) solution, and an assembly test is performed in accordance with Appendix F of GB / T 30835-2014.
[0031] In some embodiments, the carbon nanotube-polyaniline-Prussian blue analog composite material has a structure in which carbon nanotubes are branches and Prussian blue analog / polyaniline nanosheets are coated on the outside. The Prussian blue analogs are coated with polyaniline layers between the Prussian blue analogs and on their surfaces, so that the Prussian blue analogs and polyaniline form a three-dimensional sheet structure, so that adjacent Prussian blue analog nanosheets are connected to each other.
[0032] The carbon nanotube-polyaniline-Prussian blue analogue composite material adopts such a structure, has good stability, and the Prussian blue analogue is evenly distributed therein, has improved capacitance performance and charge transfer performance, and can be used as a positive electrode active material for potassium ion batteries with high capacity, high rate performance and long cycle life.
[0033] The aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material may contain other components, such as graphene, in addition to carbon nanotubes, polyaniline and Prussian blue analog as main components.
[0034] [Preparation method of carbon nanotube-polyaniline-Prussian blue analog composite material]
[0035] The preparation method of the carbon nanotube-polyaniline-Prussian blue analog composite material comprises the following steps:
[0036] Preparation process of reaction solution A: dissolving soluble divalent manganese salt and potassium citrate in deionized water, then adding N-methylpyrrolidone and polyaniline, and dispersing them evenly to form reaction solution A;
[0037] Reaction solution B preparation process: adding methanol and carbon nanotube N,N-dimethylacetamide solution to potassium ferrocyanide aqueous solution and dispersing them evenly to form reaction solution B;
[0038] Co-deposition step: the reaction solution B is mixed with the reaction solution A and heated to perform co-deposition, thereby generating a carbon nanotube-polyaniline-Prussian blue analog composite material.
[0039] In the step of preparing the reaction solution A, the concentration of the potassium citrate may be, for example, 0.1 to 0.3 mmol / mL.
[0040] In the step of preparing the reaction solution A, the soluble divalent manganese salt may be, for example, MnCl2, MnF2, MnBr2, etc., preferably MnCl2. The molar ratio of manganese ions in the soluble divalent manganese salt to the N-methylpyrrolidone may be 0.1 to 0.5:10.
[0041] In the aforementioned step of preparing the reaction solution A, the added polyaniline may be conductive polyaniline, intrinsic polyaniline, etc., preferably conductive polyaniline. Considering the charge transfer, the conductivity of the conductive polyaniline is preferably in the range of 1.0 to 2.5 s / cm. In the aforementioned step of preparing the reaction solution A, the concentration of the added polyaniline may be, for example, in the range of 1.0 to 5.0 mg / mL.
[0042] In the step of preparing the reaction solution B, the concentration of potassium ferrocyanide in the potassium ferrocyanide aqueous solution is, for example, 0.10 to 0.50 mmol / mL, the volume ratio of the added methanol to the potassium ferrocyanide aqueous solution is, for example, in the range of 1:1 to 2, and the mass ratio of the carbon nanotubes to the potassium ferrocyanide is in the range of 0.5 to 5:1000. The concentration of carbon nanotubes in the N,N-dimethylacetamide solution of carbon nanotubes is, for example, in the range of 0.1 to 0.5 mg / mL.
[0043] In the aforementioned co-precipitation process, after the reaction solution A and the reaction solution B are mixed, the Prussian blue analog complex precipitation reaction rapidly nucleates and grows, and the amine or imine group on the surface of the polyaniline is used as a template to induce the Prussian blue analog crystal to grow in a specific direction to form a lamellar crystal structure. Thus, a structure in which the molecular chains of polyaniline and the Prussian blue analog are interconnected is formed, which has good stability and uniform distribution of the Prussian blue analog, has improved capacitance performance and charge transfer performance, and can be used as a positive electrode active material for potassium ion batteries with high capacity, high rate performance and long cycle life.
[0044] In the above-mentioned co-precipitation step, the reaction temperature may be, for example, in the range of 50 to 90°C, and preferably 80 to 90°C in order to obtain a nano-sized Prussian blue analog structure.
[0045] In some embodiments of the preparation method of the carbon nanotube-polyaniline-Prussian blue analog composite material, in the aforementioned co-deposition step, the volume ratio of the mixed aforementioned reaction solution A and the aforementioned reaction solution B can be, for example, in the range of 1 to 4:1. In order to obtain a structurally stable Prussian blue analog, it is preferably in the range of 1 to 2:1, and most preferably in the range of 1 to 1.2:1.
[0046] In some embodiments, the method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material further includes the following steps:
[0047] Modification process: the carbon nanotube-polyaniline-Prussian blue analog composite material obtained in the above co-precipitation process is treated in an ice bath in 5-sulfosalicylic acid dihydrate for modification, and then washed with deionized water and dried.
[0048] Through the aforementioned modification process, an ice bath treatment is carried out in 5-sulfosalicylic acid dihydrate. Under the condition of keeping the molecular stability of sulfosalicylic acid under ice bath conditions, 5-sulfosalicylic acid is doped onto the surface of the carbon nanotube-polyaniline-Prussian blue analog composite material, thereby further improving the conductivity of the composite material.
[0049] In the aforementioned modification step, in order to introduce sulfonic acid groups on the surface of the Prussian blue analog to improve conductivity, the concentration of 5-sulfosalicylic acid dihydrate may preferably be, for example, 0.1 to 0.5 g / mL.
[0050] The above-mentioned deionized water washing can be repeated for multiple times without any particular limitation. After the deionized water washing, the substrate can be dried by heating or the like.
[0051] [Potassium ion battery positive electrode material]
[0052] The positive electrode material for potassium ion battery of the present invention comprises the aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material, or a material prepared according to the aforementioned method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material.
[0053] The positive electrode material for potassium ion battery of some embodiments includes the aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material and a substrate as a collector, wherein the aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material is attached to the surface of the aforementioned collector substrate. As the aforementioned substrate, there is no particular limitation, and it can be, for example, aluminum foil, carbon-coated aluminum foil, etc. Depending on the material used for the aforementioned substrate, when a flexible material is used as the substrate, the aforementioned electrode can be a flexible electrode.
[0054] The aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material can be coated on the surface of the aforementioned substrate to form a coating such as a thin film by coating. Furthermore, as a material coated on the aforementioned substrate, in addition to the carbon nanotube-polyaniline-Prussian blue analog composite material, it can also contain other components, such as polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC) / styrene-butadiene rubber (SBR) and other adhesives, Super P carbon black, acetylene carbon black, Ketjen black, conductive graphite and other conductive additives, N-methylpyrrolidone (NMP), N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and other solvents, etc.
[0055] Furthermore, the reversible capacity of the aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material in the potassium ion half-cell is 140-160 mAh / g (at 0.2C) and 90-100 mAh / g (at 2C), and the capacitance retention rate is greater than or equal to 92% after 500 cycles of charge and discharge at 2C.
[0056] [Potassium ion battery]
[0057] The potassium ion battery of some embodiments contains the aforementioned positive electrode material for potassium ion battery, or contains a composite material prepared by the aforementioned method for preparing a carbon nanotube-polyaniline-Prussian blue analog composite material as a positive electrode material for potassium ion battery.
[0058] In addition, the battery also has other components such as a negative electrode, a separator, an electrolyte, etc. There is no particular limitation on these components, and those skilled in the art can appropriately set them as needed.
[0059] [Application of carbon nanotube-polyaniline-Prussian blue analog composite materials in the preparation of electrodes for potassium ion batteries]
[0060] The aforementioned carbon nanotube-polyaniline-Prussian blue analog composite material or the carbon nanotube-polyaniline-Prussian blue analog composite material obtained according to the aforementioned method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material can be used as a positive electrode active material to prepare a positive electrode material for a potassium ion battery. The positive electrode material for a potassium ion battery using such a composite material has improved capacitance performance and charge transfer performance.
[0061] Example
[0062] Example 1
[0063] The carbon nanotube-polyaniline-Prussian blue analog composite was prepared by the following steps:
[0064] (1) Preparation of reaction solution A: 0.1 mmol / mL of MnCl2 and 0.2 mmol / mL of potassium citrate were dissolved in 35 mL of deionized water and magnetically stirred for 30 minutes to obtain a colorless and transparent mixed solution; 0.25 mol of N-methylpyrrolidone was added to the mixed solution, followed by 2.0 mg / mL of polyaniline, and the mixture was stirred for 12 hours.
[0065] (2) Preparation of reaction solution B: Potassium ferrocyanide was dissolved in 35 mL of deionized water under magnetic stirring to form a 0.2 mmol / mL solution, and then 25 mL of methanol was added to form a 60 mL mixed solution. Subsequently, 2.5 mL of N,N-dimethylacetamide solution containing 4 mg / mL multi-walled carbon nanotubes was added and stirred for 1 hour.
[0066] (3) Reaction solution A and reaction solution B were heated to 85° C., reaction solution A was stirred at 500 rpm, and reaction solution B was added dropwise during stirring, with the volume ratio of reaction solution A to reaction solution B being 1:1, and the mixture was stirred and mixed for 1 hour.
[0067] (4) Then, 0.125 g / mL of 5-sulfosalicylic acid dihydrate was added to the reaction solution, and the mixture was stirred for 6 hours in an ice bath. The prepared product was washed with deionized water, centrifuged, and dried at 60 degrees Celsius for 24 hours to obtain a carbon nanotube-polyaniline-Prussian blue analog composite material 1. The scanning electron microscope photograph of the obtained composite material 1 is shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the composite material 1 is in a sheet-like structure as a whole.
[0068] 8 parts by mass of composite material 1 and 1 part by mass of conductive carbon black were dispersed in a solution of 1 part by mass of polyvinylidene fluoride dissolved in 17 parts by mass of methyl pyrrolidone, and stirred for 3 hours. The completely dispersed slurry was applied on aluminum foil with a thickness of about 20 μm, and then dried at 120° C. for 24 hours to prepare electrode 1.
[0069] Using 1.0 mol / L potassium hexafluorophosphate solution as the electrolyte solution and a mixed solution of ethylene carbonate and diethyl carbonate with a volume ratio of 1:1 as the solvent, the prepared electrode material was subjected to the parameters described in the embodiment to measure the first charge capacity and cycle retention rate of the electrode 1 prepared above. The results are shown in Figure 2 , Figure 3 .from Figure 2 It can be seen that the first charge capacity of electrode 1 at 0.5C reaches 129 mAh / g, and the first discharge capacity is as high as 118 mAh / g when the discharge rate is 0.5C, indicating that the electrode material has high storage performance. Figure 3 Figure 2 is a capacity graph of 100 cycles at 0.2C, 0.5C, 1C and 2C discharge rates. Figure 3 It can be seen that electrode 1 has excellent high-speed performance and cycle stability. After cycling 100 times at 0.2C, 0.5C and 1C respectively, and a total of 300 charge and discharge cycles, the capacity at a high rate of 2C is still maintained at 108 mAh / g. After cycling 100 times at 0.2C, 0.5C, 1C and 2C respectively, and a total of 400 cycles, it returns to 0.2C and charges and discharges for another 100 cycles. After a total of 500 cycles, the capacity retention rate is still 88.7% compared to the initial capacity at 0.2C, showing excellent stability.
[0070] Comparative Example 1
[0071] The same procedure as in Example 1 was followed except that polyaniline was not added to prepare a Prussian blue analog / carbon nanotube composite material 2. The scanning electron microscope image of the composite material 2 is shown in FIG. Figure 4 As shown by Figure 4 It can be seen that it is in the form of particles with a size of 20 to 100 nm.
[0072] Under the same conditions as in Example 1, the electrode 2 was prepared using the aforementioned Prussian blue analogue / carbon nanotube composite material 2 .
[0073] The impedance spectra of electrode 1 and electrode 2 are as follows Figure 5 As shown. The surface contact resistance of electrode 2 without polyaniline is about 27.2Ω, which is 5.9 times that of electrode 1 with polyaniline. ct , electrode 2 is about 5420Ω, which is about 6 times that of electrode 1. Figure 5 It can be seen from the comparison that the conductivity of the material can be greatly improved by using a carbon nanotube-polyaniline-Prussian blue analog composite material with added polyaniline.
[0074] The performance of electrode 2 was measured, and the results were as follows: Figure 6 As shown, the first charge capacity is 114 mAh / g and the discharge capacity is 101 mAh / g, which is much lower than that of electrode 1.
[0075] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0076] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0077] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a carbon nanotube-polyaniline-Prussian blue analogue composite material, wherein the carbon nanotube-polyaniline-Prussian blue analogue composite material comprises carbon nanotubes, Prussian blue analogues attached to the surface of the carbon nanotubes, and polyaniline connecting the Prussian blue analogues to each other. The preparation method of the carbon nanotube-polyaniline-Prussian blue analog composite material comprises the following steps: Preparation process of reaction solution A: dissolving soluble divalent manganese salt and potassium citrate in deionized water, then adding N-methylpyrrolidone and polyaniline, and dispersing them evenly to form reaction solution A; Reaction solution B preparation process: adding methanol and carbon nanotube N,N-dimethylacetamide solution to potassium ferrocyanide aqueous solution and dispersing them evenly to form reaction solution B; Co-deposition step: the reaction solution B is mixed with the reaction solution A and heated to perform co-deposition, so as to generate a carbon nanotube-polyaniline-Prussian blue analog composite material.
2. The method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material according to claim 1, further comprising the following steps: Modification process: the carbon nanotube-polyaniline-Prussian blue analog composite material obtained in the co-precipitation process is treated in an ice bath in 5-sulfosalicylic acid dihydrate for modification, and then washed with deionized water and dried, wherein the concentration of the 5-sulfosalicylic acid dihydrate is 0.1-0.5 g / mL.
3. According to the method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material according to claim 1, in the step of preparing the reaction solution A, the concentration of the potassium citrate is 0.1-0.3 mmol / mL, the soluble divalent manganese salt is MnCl2, the molar ratio of MnCl2 to the N-methylpyrrolidone is 0.1-0.5:10, and the total concentration of the added polyaniline is 1.0-5.0 mg / mL.
4. The method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material according to claim 1, wherein: In the step of preparing the reaction solution B, the concentration of potassium ferrocyanide in the potassium ferrocyanide aqueous solution is 0.10 to 0.50 mmol / mL. The volume ratio of the added methanol to the potassium ferrocyanide aqueous solution is 1:1-2, the mass ratio of the carbon nanotubes to the potassium ferrocyanide is 0.5-5:1000, and the concentration of the carbon nanotubes in the N,N-dimethylacetamide solution of the carbon nanotubes is 0.1-0.5 mg / mL.
5. The method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material according to claim 1, wherein: In the co-deposition process, the reaction temperature is 80-90° C., and the volume ratio of the reaction solution A to the reaction solution B is 1-4:
1.
6. The method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material according to claim 1, wherein: The Prussian blue analogue is a sheet structure with a size of 20 to 100 nm, the carbon nanotube is a multi-walled carbon nanotube with a diameter of 10 to 50 nm, and the polyaniline is a sheet structure with a thickness of 100 to 200 nm and a size of 500 nm to 1 μm.
7. The method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material according to claim 1, wherein: The reversible capacity of the carbon nanotube-polyaniline-Prussian blue analog composite material is 140-160 mAh / g at 0.2C and 90-100 mAh / g at 2C.
8. A positive electrode material for a potassium ion battery, comprising the carbon nanotube-polyaniline-Prussian blue analogue composite material obtained by the method for preparing the carbon nanotube-polyaniline-Prussian blue analogue composite material according to any one of claims 1 to 7. 9 . A potassium ion battery comprising the positive electrode material for a potassium ion battery according to claim 8 .
10. Use of the carbon nanotube-polyaniline-Prussian blue analog composite material obtained by the method for preparing the carbon nanotube-polyaniline-Prussian blue analog composite material according to any one of claims 1 to 7 in preparing a cathode material for a potassium ion battery.