A method for resource utilization of smelting slag

By uniformly mixing lead sludge, garbage fly ash and compound materials in the slag furnace, forming mineral wool melt and fibers, the problem of low resource utilization value of lead sludge is solved, and efficient lead sludge and The coordinated utilization of garbage fly ash reduces energy consumption and improves heavy metal recovery.

CN115838247BActive Publication Date: 2024-11-12HUNAN RE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211213226.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-12
Estimated Expiration
2042-09-30

Smart Images

  • Figure CN115838247B_ABST
    Figure CN115838247B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for resource utilization of smelting slag, wherein the smelting slag melt to be processed is input into a slag furnace through a chute; at the same time, garbage fly ash and batch material powder are added into the chute, so that the garbage fly ash and batch material powder flow into the slag furnace together with the smelting slag melt, and are smelted to obtain a mineral wool melt and flue gas; wherein the ingredients of the batch material include one or more of CaO, MgO, SiO2, Al2O3, and chloride; and cotton fiber is prepared using the mineral wool melt as a raw material. The present invention can simply and efficiently achieve full mixing of the smelting slag melt and the batch material powder by controlling the chute and the timing of adding the garbage fly ash and batch material powder. At the same time, when the smelting slag melt and the batch material powder in the chute fall into the slag furnace, they have a strong impact and stirring effect on the existing melt, which helps to strengthen mass transfer and heat transfer, ensure the treatment effect, and improve the treatment efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for resource utilization of smelting slag, and belongs to the technical field of resource utilization of solid waste. Background Art

[0002] Both the reduction smelting of lead and the fuming furnace smelting of the reduction smelting slag will produce a large amount of slag, of which the slag of the reduction smelting contains about 2% lead, and the slag of the fuming furnace smelting contains about 0.5% lead. The lead content in both slags exceeds the limit value in the "Identification of Hazardous Waste Identification Standard Leaching Toxicity Identification" (GB 5085.3-2007). In addition, heavy metals such as zinc and cadmium will remain in both slags due to different raw materials. In order to reduce the leaching toxicity of the slag, water quenching is currently generally used to rapidly cool the high-temperature hot slag to form glassy water-quenched slag, and lead, cadmium, zinc, etc. are sealed in the water-quenched slag. The metal content in the water-quenched slag is low and dispersed, and it is difficult to purify or the purification is not economical. Therefore, the water-quenched slag has become the main solid waste of lead smelters and is currently mainly used in the field of building materials. For example, Chinese invention patent application CN114057415A discloses a multi-solid waste gel material, a multi-solid waste filling material based on the gel material, and its preparation method and application, wherein lead smelting water quenching slag powder, cement clinker powder, slag powder, ash slag, ammonia evaporation waste slag, full-grade tailings, and water are mixed in proportion and synergistically excited to prepare ecological filling materials with different slurry concentrations, different strengths, and different slumps. In addition, lead smelting slag contains cotton fiber components such as SiO2, Fe2O3, Al2O3, and CaO, but the component ratio cannot or is difficult to directly form cotton fibers with higher application value.

[0003] Mineral wool is a man-made high-quality thermal insulation material, widely used in many fields such as construction and industry. Rock mineral wool is a thermal insulation material produced with basalt, slag and other raw materials, and is mostly used for thermal insulation of walls and pipes. With the advancement of rock mineral wool production technology and the development of resource recycling economy, the production of rock mineral wool with industrial solid waste such as slag and tailings instead of natural rock and mineral raw materials has become an important development direction of the industry, and related products have also been recognized by the market. Compared with building materials such as gel materials and filling materials, rock wool has a higher value and is an important direction for realizing high-value utilization of water-quenched slag, especially the direct utilization of hot slag. For example, Chinese patent application CN104529147A discloses a method for producing mineral wool fibers using high-temperature hot waste slag from a metallurgical furnace as raw material, and using waste slag from the smelting of copper, nickel, lead, zinc, tin and iron to produce mineral wool fibers. In this patent application, limestone, quartz stone or a mixture of the two is used as a tempering agent, and 85%-100% of the hot waste slag and 0%-15% of the tempering agent are melted and stirred homogenized in an insulating electric furnace, and then a four-roll centrifuge is used to form fibers to obtain mineral wool fibers. However, it does not involve the treatment of residual metals in the smelting slag, and the residual metals in the smelting slag cannot be reasonably utilized; in addition, the mixing of the tempering agent and the hot waste slag is completely carried out in a thermal insulation electric furnace, and homogenization is achieved by stirring. The stirring of high-temperature melts is difficult to achieve large-scale industrial production. Summary of the invention

[0004] In view of the deficiencies of the prior art, an object of the present invention is to provide a method for resource utilization of smelting slag, so as to utilize the smelting slag as a resource in a simpler and more efficient manner.

[0005] In order to solve the above technical problems, the technical solution of the present invention is as follows:

[0006] A method for resource utilization of smelting slag comprises the following steps:

[0007] S1. The smelting slag melt to be processed is fed into the slag furnace through a chute; at the same time, garbage fly ash and batch materials are added into the chute, so that the garbage fly ash and batch materials flow into the slag furnace together with the smelting slag melt, and are smelted to obtain mineral wool melt and flue gas;

[0008] Wherein, the ingredients of the batch material include one or more of CaO, MgO, SiO2, and Al2O3; preferably, the connection position between the chute and the slag furnace is higher than the liquid level in the slag furnace.

[0009] S2, fiberizing the mineral wool melt to obtain cotton fibers (mineral wool fibers).

[0010] In the present invention, on the one hand, the smelting slag melt is directly input into the slag furnace, which can make full use of the heat of the smelting slag melt and significantly reduce energy consumption; on the other hand, the smelting slag melt is input into the slag furnace through a chute; at the same time, the garbage fly ash and the batch material are added to the chute, so that the garbage fly ash and the batch material flow into the slag furnace together with the smelting slag melt. Since the smelting slag melt is always in a flowing state, the garbage fly ash and the batch material can be evenly spread on the surface of the melt once added to the chute, and then further flow and further mix with the smelting slag melt, and finally flow into the slag furnace together with the smelting slag melt, and then further mix, and impact the existing melt in the slag furnace, so that the melt produces relative flow. Therefore, the smelting slag melt and the garbage fly ash and the batch material of the present invention can be simply and fully mixed, and the newly added smelting slag melt and the batch material continuously impact the existing melt in the slag furnace, effectively strengthening mass transfer and heat transfer, helping to save energy consumption, and speeding up the smelting process and improving processing efficiency.

[0011] Furthermore, the maximum width of the chute is 3-6 times the long side width or diameter of the slag discharge port 1-1 of the metal smelting furnace, and the depth δ of the molten slag in the chute is maintained at 50-200 mm. Preferably, the reactor chute is U-shaped, and the melt should immerse the entire U-shaped bottom.

[0012] Furthermore, the height H of the chute is not less than 3 times the depth δ of the melt, the angle α between the chute and the vertical direction is 75-85°, and the length of the chute is adjusted according to the viscosity of the smelting slag to ensure that the melt can flow throughout the chute.

[0013] Furthermore, the smelting slag is lead smelting slag, and based on dry weight, the content of SiO2 is 25-30wt%, the content of Al2O3 is 8-12wt%, the content of Fe2O3 is 30-40wt%, the content of CaO is 10-15wt%, the content of MgO is 0-5wt%, the sum of the contents of Na2O and K2O is ≤5wt%, and the content of Pb is ≤2wt%.

[0014] Furthermore, the batch material comprises 27-32 parts of fly ash, 12-18 parts of talc, 0-8 parts of quartz powder and 0-2 parts of reducing agent in terms of dry weight. In this way, the present invention can not only solve the problem of low resource utilization value of existing lead smelting slag, but also improve the resource utilization value of lead smelting slag in a lower carbon way, while synergistically treating garbage fly ash harmlessly.

[0015] Furthermore, the compound material comprises, by dry weight, 32-38 parts of garbage fly ash, 31-34 parts of fly ash, 14-16 parts of talcum powder, 2-6 parts of quartz powder, and 0-1.8 parts of reducing agent.

[0016] Furthermore, the garbage fly ash is fly ash from incineration of domestic waste for power generation, and the talc content in the talc powder is ≥ 75wt%; preferably, the garbage fly ash is grate furnace fly ash.

[0017] Furthermore, the reducing agent is one or more of coke powder, coal powder, and waste activated carbon powder.

[0018] Furthermore, in the garbage fly ash, the CaO content is 45-50wt%, the chlorine content is 20-28wt%, the Fe2O3 content is ≤5wt%, and the total content of Na2O and K2O is ≤12wt%; in the fly ash component, the SiO2 content is 48-55wt%, the Al2O3 content is 24-30wt%, the Fe2O3 content is ≤6wt%, and the total content of Na2O and K2O is ≤6wt%; in the talc powder, the SiO2 content is 48-54wt%, and the MgO content is 25-30wt%; in the quartz powder, the SiO2 content is ≥98wt%.

[0019] Optionally, the fineness of the batch powder is ≥200 mesh.

[0020] Optionally, the fineness of the talcum powder is ≥200 mesh, and the fineness of the quartz powder is ≥200 mesh.

[0021] Lead smelting slag contains SiO2, Fe2O3, Al2O3, CaO and other components that can be used to construct cotton fibers, but the proportion of the components cannot or is difficult to form cotton fibers. By coordinating with garbage fly ash, fly ash, talcum powder and quartz powder, using garbage fly ash to supplement CaO, fly ash to supplement Al2O3 and SiO2, talcum powder to supplement MgO and SiO2, and quartz powder to supplement SiO2, the combination of the components between the materials can obtain a stable melt with suitable high-temperature viscosity characteristics, and then further through multi-roller centrifugal fiber forming and other methods to obtain cotton fibers. Garbage fly ash also contains chlorine. Under high temperature, some of the Pb and other residues in the lead smelting slag and some volatile heavy metals in the garbage fly ash are converted into chlorides and enter the flue gas, and are enriched in the flue gas. The difficult-to-volatilize heavy metals and the remaining volatile heavy metals are wrapped in the glassy high-temperature melt and fixed in the cotton fibers. Dioxins in garbage fly ash are cracked when melted at high temperature, heavy metals in lead smelting slag and garbage fly ash are fixed by cotton fibers, and a small amount of Fe2O3 is reduced in the slag furnace to form ferroalloys, which can be discharged from the iron tapping nozzle regularly to obtain ferroalloys; the smoke dust obtained from the flue gas dust collection treatment is soaked in water, and the lead-containing filtrate obtained can be used to recover lead and potassium and sodium crude salts after concentration. In the whole process, the sensible heat of hot lead smelting slag is used to achieve electric melting, and the lead lost in the lead smelting process is further recovered through the synergy of lead smelting slag and garbage fly ash. Under the joint action of fly ash, talcum powder and quartz powder, glass suitable for the production of cotton fibers is smelted to form a glass body, so that wastes such as lead smelting slag, garbage fly ash, and fly ash are used in a high-value manner. At the same time, the lead smelting slag and garbage fly ash are harmlessly treated, and the residual heavy metals are wrapped and fixed in cotton fibers. The toxic leaching value of the obtained cotton fibers meets the limit value in the "Identification of Hazardous Waste Identification Standard Leaching Toxicity Identification" (GB 5085.3-2007).

[0022] Further, the flue gas is subjected to dust collection treatment to obtain ash; the ash is then soaked in water to obtain filter residue and lead-containing filtrate; the filter residue is returned to S1 and added to the batch powder. Optionally, the filter residue is dried and crushed to a fineness of ≥200 mesh, and then added to the batch powder; wherein the addition amount is <2wt% (dry basis).

[0023] Optionally, the flue gas is first quenched and then dust is collected to avoid the re-formation of dioxins in the flue gas.

[0024] Furthermore, based on dry weight, the mass ratio of the lead smelting slag melt, garbage fly ash and batch material is 30-35:30-40:40-60, and further 31-34:32-38:45-55.

[0025] Furthermore, in S1, the smelting time is 60-120 min, further 70-110 min, and further 80-100 min.

[0026] Further, in S2, the cotton fibers are prepared by a multi-roll centrifuge. Optionally, a cotton collector is used to collect the cotton fibers for producing cotton products.

[0027] Furthermore, in S2, an adhesive must be applied during the multi-roller centrifugal fiber forming process, and the amount used is less than 4wt% of the organic matter content remaining in the cotton product; preferably, the adhesive is a composition of phenolic resin, water repellent, dust-proof oil, etc.

[0028] Furthermore, the top of the chute is provided with a plurality of feeding ports, which are sequentially distributed along the length direction of the chute; along the flow direction of the smelting slag melt in the chute, the garbage fly ash is added through the first 1-5 feeding ports, and the batch material is added through the last 1-3 feeding ports; preferably, the plurality of feeding ports are sequentially and evenly distributed along the length direction of the chute. In this way, the garbage fly ash and the batch material can be added in a dispersed manner, avoiding excessive garbage fly ash or batch material added at a single point in an instant, which may cause agglomeration or difficulty in mixing, and in particular, can improve the uniformity of mixing of the chlorine-containing substances in the garbage fly ash and the melt, and promote the formation of metal chlorides such as lead chloride.

[0029] Furthermore, the chute includes a trough body, a feed port is provided at one end of the trough body, a discharge port is provided at the other end of the trough body, and the discharge port is connected to the slag furnace; the discharge port is trumpet-shaped, the bottom surface of the discharge port is inclined, and the angle β with the vertical direction is 20-50°; preferably, the angle α between the trough body and the vertical direction is 70-85°.

[0030] Furthermore, the long side L1 of the slag discharge port is 0.4-0.6 times the width of the slag furnace, and the short side L2 of the slag discharge port is 0.4-0.6 times the long side L1.

[0031] Furthermore, in S1, the batch material is evenly spread on the surface of the molten slag in the chute.

[0032] Furthermore, the water content of each material in the batch is less than 0.5wt%.

[0033] Furthermore, in the process of leading the smelting slag melt into the slag furnace through the chute, the flow rate is measured, and the addition amount of the batch material is controlled according to the flow rate measurement result; preferably, the flow rate measurement is online real-time monitoring.

[0034] Furthermore, the chute is a closed chute, and the top of the chute is connected to the flue of the slag furnace.

[0035] Furthermore, the chute is provided with a feeding port for adding batch materials.

[0036] Optionally, in S2, the viscosity of the mineral wool melt is less than 0.5 Pa·s.

[0037] Furthermore, the slag furnace is an electric heating furnace. Optionally, the smelting slag melt inlet and the batch material feeding port are on the same side, and the slag outlet is on the other side of the lead smelting slag inlet; preferably, the slag outlet is directly opposite to the slag furnace melt inlet, which can make the high-temperature melt in the slag furnace produce more intense relative flow, further improve the uniformity of the melt, and thus improve the quality of cotton fiber.

[0038] Furthermore, the liquid level in the slag furnace must be kept higher than the highest position of the slag outlet at all times; preferably, the stable melt volume in the slag furnace is controlled to be 1-2 times the amount of smelting slag melt input at a single time.

[0039] Furthermore, when the slag furnace is started, hot smelting slag is first put into the slag furnace, then the power is turned on to increase the temperature, and then batch material is added to the slag furnace. After the slag furnace provides stable heat, the material is added according to the automatic proportion. Specifically, the batch material is spread on the surface of the smelting slag melt in the chute, so that the batch material powder flows into the slag furnace together with the smelting slag melt.

[0040] The present invention makes full use of the heat of hot smelting slag and can significantly reduce the melting energy consumption; garbage fly ash, fly ash, talcum powder, quartz powder and reducing agent are all fine powders, which are spread on the surface of hot lead smelting slag and flow into the slag furnace together, so that the batch material and the hot lead smelting slag are evenly mixed, and the melting speed is improved, which is beneficial to further energy saving; the powder is fully mixed with the hot lead smelting slag, the contact area between chlorine and the lead smelting slag is increased, the volatilization of lead chloride and the like is promoted, and the recovery rate of residual metals in the slag and fly ash can be improved.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] 1. The present invention can simply and efficiently achieve sufficient mixing of the smelting slag melt and the batch material by controlling the timing of adding the chute, garbage fly ash and batch material. At the same time, when the smelting slag melt and the batch material in the chute fall into the slag furnace, they have a strong impact on the existing melt, causing the melt to flow relatively, which helps to enhance mass transfer and heat transfer, ensure the treatment effect, and improve the treatment efficiency.

[0043] 2. The present invention uses the synergy of smelting slag and garbage fly ash. The garbage fly ash serves as a calcium source to supplement CaO in the lead smelting slag, thereby promoting the lead smelting slag to form a stable glass body; the Cl in the garbage fly ash reacts with residual volatile metals such as lead to form volatile chlorides that enter the smoke and are enriched and recovered; the non-volatile heavy metals and a small amount of residual volatile heavy metals are wrapped and fixed by the glassy melt, thereby reducing the loss of metals in the lead smelting slag and improving the value of resource utilization.

[0044] 3. The present invention utilizes smelting slag in coordination with garbage fly ash, fly ash, etc. to melt and form a high-temperature melt that can be used to produce rock wool fibers. The leaching toxicity of the obtained cotton fibers meets the limit value, and the product value is relatively high.

[0045] 4. The present invention directly utilizes the hot lead smelting slag melt, avoiding a large amount of heat loss caused by water quenching. Compared with converting it into water-quenched slag for reuse, it has the advantage of significantly reducing production energy consumption. At the same time, it can use the hot lead smelting slag as a conductive medium to start the slag furnace, which can significantly increase the furnace starting speed and reduce the furnace starting energy consumption.

[0046] 5. In the present invention, the batch material and the hot smelting slag are simultaneously introduced into the slag furnace, which accelerates the homogenization of the melt and improves the uniformity, which is beneficial to the improvement of the quality of cotton fiber forming and reduces the slag ball content in the cotton fiber. At the same time, the contact area between chlorine and lead smelting slag is increased, which promotes the volatilization of lead chloride and the like, and can improve the recovery rate of residual metals in slag and fly ash.

[0047] 6. The total disposal capacity of solid waste and hazardous waste in the present invention reaches more than 80%, which can effectively reduce the use of natural mineral raw materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 It is a schematic cross-sectional view of the chute of the present invention.

[0049] Figure 2 It is a schematic plan view of the chute of the present invention.

[0050] Figure 3 It is a schematic diagram of the cross section of the chute of the present invention.

[0051] In the figure: 1-reaction furnace; 2-chute; 3-slag furnace; 11-material layer; 12-liquid surface; 13-liquid slag layer. DETAILED DESCRIPTION

[0052] The present invention will be described in detail below in conjunction with the embodiments. It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present invention can be combined with each other. Unless otherwise specified, the relevant percentages refer to mass percentages.

[0053] The raw material components used in the embodiments and comparative examples of the present invention are shown in Table 1. The lead smelting slag is the slag of the lead reduction furnace; the talc content in the talc powder is 80.1wt%; and the quartz content in the quartz powder is 98.5wt%.

[0054] Table 1

[0055]

[0056] Example 1

[0057] A method for resource utilization of lead smelting slag, such as Figure 1-Figure 3 As shown, the specific steps include:

[0058] According to the dry weight, 29 parts of fly ash, 15 parts of talcum powder, 4 parts of quartz powder and 1 part of coal powder are pneumatically mixed to obtain a batch material; 35 parts of garbage fly ash are taken for standby use. Among them, the garbage fly ash is the grate furnace fly ash of the domestic waste power plant; the fineness of talcum powder is -200 mesh; the fineness of quartz powder is -200 mesh; the fineness of fly ash is -200 mesh.

[0059] A slag discharge port 1-1 is provided on the side of the reaction furnace 1, and the slag discharge port 1-1 is a circular port with a diameter of 100 mm. The reaction furnace 1 is a lead reduction furnace. The chute has a feed port and a discharge port 3-1, and the feed port is connected to the slag discharge port 1-1. The cross section of the slag furnace 3 is rectangular, and the discharge port 3-1 is connected to the slag furnace 3. The connection position between the discharge port 3-1 and the slag furnace 3 and the slag discharge port are arranged on both sides of the short side of the slag furnace 3. The chute 2 is U-shaped, with an angle α of 80° with the vertical direction, a width B of 400mm, a height H of 500mm, and an internal melt depth of 150±10mm (the distance between the melt surface and the lowest point of the bottom of the chute); the discharge port 3-1 is trumpet-shaped, the length L1 of the discharge port 3-1 is 0.5 times the width of the slag furnace 3, the width L2 of the discharge port 3-1 is half of the length L1, the bottom surface of the discharge port 3-1 is inclined, and the angle β with the vertical direction is 30°. A feed port 2-A with a diameter of 400mm is provided at the top of the discharge port 3-1; the top of the chute 2 is provided with three feed ports 2-B1, 2-B2, and 2-B3 distributed in sequence along the length direction, with a spacing a=b=c, and the diameters of the feed ports 2-B1, 2-B2, and 2-B3 are 200mm.

[0060] The hot lead smelting slag melt in the lead reduction furnace (reaction furnace 1) flows into the slag furnace through the chute 2, and the batch material in the front silo is quantitatively added from the charging port on the chute 2, spread on the surface of the hot lead smelting slag melt and enter the slag furnace together with the slag, and smelt for 90 minutes to obtain mineral wool melt and flue gas. The proportion of lead smelting slag and batch material is automatically controlled, that is, the slag discharge amount is pre-set according to 32 parts by weight of lead smelting slag melt, 48 parts by weight of batch material, and 35 parts by weight of garbage fly ash, and then the amount of batch material is calculated. After the batch material is weighed, a screw feeder is used to quantitatively add the material to the charging port on the chute, wherein 48 parts of batch material are added from the charging port 2-A, and 10 parts by weight, 12 parts by weight, and 13 parts by weight of garbage fly ash are added from the charging ports 2-B1, 2-B2, and 2-B3, respectively.

[0061] The flue gas is first cooled to 200°C by a heat exchanger, and then the flue gas is purified to obtain flue dust. The flue dust contains 0.85% lead and the lead recovery rate is 58.40%. The obtained flue dust is leached with soft water to obtain filtrate and filter residue, which is dried and ground to 200 mesh and added to the batch material in an amount of 1wt%; the filtrate is concentrated and caustic alkali is added to precipitate lead, and crude salt is obtained by evaporation and crystallization.

[0062] The slag furnace maintains a stable melt of 1.5±0.1 times the single slag discharge amount of the lead reduction furnace, controls the temperature in the slag furnace to 1500±25°C, makes the viscosity of the mineral wool melt at the slag outlet to 0.4±0.1Pa·s, feeds the mineral wool melt into a four-roll centrifuge, and forms fibers to obtain cotton fibers with an average diameter of 5.5μm and a slag ball content of 5.53%, wherein a composite binder such as phenolic resin, water repellent, and dustproof oil is applied during the fiber forming process. The leaching toxicity of the cotton fiber meets the limit value in the "Identification of Hazardous Waste Identification Standard Leaching Toxicity Identification" (GB 5085.3-2007).

[0063] Comparative Example 1

[0064] Example 1 was repeated, with the only difference being that there was no feed port on the chute, and the batch material and garbage fly ash were directly fed into the slag furnace.

[0065] The material layer of the batch material gathered and floated on the surface of the melt, and part of the material layer was still not melted after smelting for 90 minutes; the obtained smoke contained 0.52% lead and the recovery rate was 35.53%; the amount of slag balls produced in the fiber forming process was 6.78%.

[0066] Comparative Example 2

[0067] Example 1 is repeated, except that only a feed port 2-A is provided on the chute, and garbage fly ash is mixed with the batch material and fed in from the feed port 2-A.

[0068] After the batch material is added, it first accumulates at the discharge port, and is dispersed with the inflow of lead smelting slag, and dispersed into the slag furnace. After smelting for 90 minutes, the material layer is basically melted. The obtained smoke contains 0.67% lead, and the recovery rate is 46.20%; the amount of slag balls produced during the fiber forming process is 5.99wt%.

[0069] Comparative Example 3

[0070] Example 1 was repeated, with the only difference being that one feeding port 2-A and one feeding port 2-B were provided on the chute; 48 parts of batch material were added through the feeding port 2-A, and 35 parts of garbage fly ash were added through the feeding port 2-B.

[0071] After the batch material is added, it first accumulates at the discharge port, and the accumulation height decreases. With the inflow of lead smelting slag, it is dispersed into the slag furnace. After smelting for 90 minutes, the material layer melts. The obtained smoke contains 0.74% lead, and the recovery rate is 51.18%. There is no obvious change in the amount of slag balls produced during the fiberization process.

[0072] Comparative Example 4

[0073] Example 1 is repeated, with the only difference being that: garbage fly ash is mixed into the batch material to form a mixture; and the mixture is added through the feed port 2-A and the feed port 2-B.

[0074] The obtained smoke contains 0.72% lead and the recovery rate is 49.33%. The amount of slag balls produced in the fiber-forming process is slightly reduced.

[0075] It can be seen that when the batch materials are directly added to the slag furnace, the mixing effect between the silo and the melt is poor, the volatilization of lead is reduced, and the uniformity of the mineral wool melt also deteriorates. Mixing garbage fly ash into the batch materials can slightly improve the uniformity of the melt, but is not conducive to the volatilization of lead.

[0076] Comparative Example 5

[0077] Example 1 was repeated, except that the width B was 550 mm and the internal melt depth was 35±10 mm.

[0078] The results showed that part of the lead smelting slag had solidified when it flowed into the melt, causing batch material to remain in the chute.

[0079] Example 2

[0080] A method for resource utilization of lead smelting slag, specifically comprising the following steps:

[0081] According to the dry weight, 27 parts of fly ash, 12 parts of talcum powder, 6 parts of quartz powder, 0.5 parts of coal powder and 0.5 parts of waste activated carbon powder are pneumatically mixed to obtain a batch material; 40 parts of garbage fly ash are taken for standby use. Among them, the garbage fly ash is the grate furnace fly ash of the domestic waste power plant; the fineness of talcum powder is -200 mesh; the fineness of quartz powder is -200 mesh; the fineness of fly ash is -200 mesh.

[0082] A slag discharge port 1-1 is provided on the side of the reaction furnace 1, and the slag discharge port 1-1 is a circular port with a diameter of 100 mm. The reaction furnace 1 is a lead reduction furnace. The chute has a feed port and a discharge port 3-1, the feed port is connected to the slag discharge port 1-1, the cross section of the slag furnace 3 is rectangular, the discharge port 3-1 is connected to the slag furnace 3, and the connection position between the discharge port 3-1 and the slag furnace 3 and the slag discharge port are arranged on both sides of the short side of the slag furnace 3. The chute 2 is U-shaped, with an angle α of 75° with the vertical direction, a width B of 400 mm, a height H of 500 mm, and an internal melt depth of 80±10 mm; the discharge port 3-1 is trumpet-shaped, the length L1 of the discharge port 3-1 is 0.4 times the width of the slag furnace 3, the width L2 of the discharge port 3-1 is half the length L1, and the bottom surface of the discharge port 3-1 is inclined, and the angle β with the vertical direction is 45°. A feeding port 2-A with a diameter of 400 mm is provided at the top of the discharge port 3-1; two feeding ports 2-B1 and 2-B2 are provided at the top of the chute 2, which are distributed in sequence along the length direction, with a spacing of a=b=c, and the diameters of the feeding ports 2-B1 and 2-B2 are both 200 mm.

[0083] The hot lead smelting slag melt in the lead reduction furnace (reaction furnace 1) flows into the slag furnace through the chute 2, and the batch material in the front of the furnace is quantitatively added from the charging port on the chute 2, spread on the surface of the hot lead smelting slag melt and enter the slag furnace together with the slag, and smelt for 80 minutes to obtain mineral wool melt and flue gas. The proportion of lead smelting slag and batch material is automatically controlled, that is, the slag discharge amount is pre-set according to 30 parts by weight of lead smelting slag melt, 46 parts by weight of batch material, and 40 parts by weight of garbage fly ash, and then the amount of batch material is calculated. After the batch material is weighed, a screw feeder is used to quantitatively add the material to the charging port on the chute, wherein 46 parts of batch material are added from the charging port 2-A, and 15 parts by weight, 25 parts by weight, and 13 parts by weight of garbage fly ash are added from the charging port 2-B1 and the charging port 2-B2, respectively.

[0084] The flue gas is first cooled to 200°C by a heat exchanger, and then the flue gas is purified to obtain flue dust. The flue dust contains 0.68% lead and the lead recovery rate is 57.22%. The obtained flue dust is leached with soft water to obtain filtrate and filter residue, which is dried and ground to 200 mesh and added to the batch material in an amount of 2wt%; the filtrate is concentrated and caustic alkali is added to precipitate lead, and crude salt is obtained by evaporation and crystallization.

[0085] The slag furnace maintains a stable melt of 1.2±0.1 times the single slag discharge amount of the lead reduction furnace, controls the temperature in the slag furnace to 1480±25℃, makes the viscosity of the mineral wool melt at the slag outlet to 0.3±0.1Pa·s, feeds the mineral wool melt into a four-roll centrifuge, and forms fibers to obtain cotton fibers with an average diameter of 5.1μm, wherein a composite binder such as phenolic resin, water repellent, and dustproof oil is applied during the fiber forming process. The leaching toxicity of the cotton fiber meets the limit value in the "Identification of Leaching Toxicity of Hazardous Waste Identification Standard" (GB 5085.3-2007).

[0086] Example 3

[0087] A method for resource utilization of lead smelting slag, specifically comprising the following steps:

[0088] According to the dry weight, 32 parts of fly ash and 18 parts of talcum powder are pneumatically mixed to obtain a batch material; 30 parts of garbage fly ash are taken for standby use. The garbage fly ash is the grate furnace fly ash of the domestic waste power plant; the fineness of the talcum powder is -200 mesh; the fineness of the fly ash is -200 mesh.

[0089] A slag discharge port 1-1 is provided on the side of the reaction furnace 1, and the slag discharge port 1-1 is a circular port with a diameter of 100 mm. The reaction furnace 1 is a lead reduction furnace. The chute has a feed port and a discharge port 3-1, the feed port is connected to the slag discharge port 1-1, the cross section of the slag furnace 3 is rectangular, the discharge port 3-1 is connected to the slag furnace 3, and the connection position between the discharge port 3-1 and the slag furnace 3 and the slag discharge port are arranged on both sides of the short side of the slag furnace 3. The chute 2 is U-shaped, with an angle α of 85° with the vertical direction, a width B of 350 mm, a height H of 600 mm, and an internal melt depth of 190±10 mm; the discharge port 3-1 is trumpet-shaped, the length L1 of the discharge port 3-1 is 0.6 times the width of the slag furnace 3, the width L2 of the discharge port 3-1 is half the length L1, and the bottom surface of the discharge port 3-1 is inclined, and the angle β with the vertical direction is 45°. A square feeding port 2-A with a side length of 450 mm is provided at the top of the discharge port 3-1; two feeding ports 2-B1 and 2-B2 are provided at the top of the chute 2, which are distributed in sequence along the length direction, with a spacing of a=b=c. Both the feeding ports 2-B1 and 2-B2 are square with a side length of 150 mm.

[0090] The hot lead smelting slag melt in the lead reduction furnace (reaction furnace 1) flows into the slag furnace through the chute 2, and the batch material in the front of the furnace is quantitatively added from the feeding port on the chute 2, spread on the surface of the hot lead smelting slag melt and enter the slag furnace together with the slag, and smelt for 120 minutes to obtain mineral wool melt and flue gas. The proportion of lead smelting slag and batch material is automatically controlled, that is, the slag discharge amount is pre-set according to 35 weight parts of lead smelting slag melt, 50 weight parts of batch material, and 30 weight parts of garbage fly ash, and then the amount of batch material is calculated. After the batch material is weighed, a screw feeder is used to quantitatively feed it to the feeding port on the chute, wherein 50 parts of batch material are added from the feeding port 2-A, and 10 parts of garbage fly ash are added from the feeding port 2-B1 and the feeding port 2-B2, respectively.

[0091] The flue gas is first cooled to 200°C by a heat exchanger, and then the flue gas is purified to obtain flue dust. The flue dust contains 1.04% lead, and the lead recovery rate is 56.24%. The obtained flue dust is leached with soft water to obtain filtrate and filter residue, which is dried and ground to 200 mesh and added to the batch material at a dosage of 0.5wt%; the filtrate is concentrated and caustic alkali is added to precipitate lead, and crude salt is obtained by evaporation and crystallization.

[0092] The slag furnace maintains a stable melt of 1.8±0.1 times the single slag discharge amount of the lead reduction furnace, controls the temperature in the slag furnace to 1520±25℃, makes the viscosity of the mineral wool melt at the slag outlet to 0.4±0.1Pa·s, feeds the mineral wool melt into a four-roll centrifuge, and forms fibers to obtain cotton fibers with an average diameter of 5.2μm, wherein a composite binder such as phenolic resin, water repellent, and dustproof oil is applied during the fiber forming process. The leaching toxicity of the cotton fiber meets the limit value in the "Identification of Hazardous Waste Identification Standard Leaching Toxicity Identification" (GB 5085.3-2007).

[0093] Example 4

[0094] A method for resource utilization of lead smelting slag, specifically comprising the following steps:

[0095] According to the dry weight, 28 parts of fly ash, 12 parts of talcum powder and 8 parts of quartz powder are pneumatically mixed to obtain a batch material; 36 parts of garbage fly ash are taken for standby use. The garbage fly ash is the grate furnace fly ash of the domestic waste power plant; the fineness of the talcum powder is -200 mesh; the fineness of the fly ash is -200 mesh; the fineness of the quartz powder is -300 mesh, and the quartz content is 99.0wt%.

[0096] A slag discharge port 1-1 is provided on the side of the reaction furnace 1, and the slag discharge port 1-1 is a circular port with a diameter of 100 mm. The reaction furnace 1 is a lead reduction furnace. The chute has a feed port and a discharge port 3-1, the feed port is connected to the slag discharge port 1-1, the cross section of the slag furnace 3 is rectangular, the discharge port 3-1 is connected to the slag furnace 3, and the connection position between the discharge port 3-1 and the slag furnace 3 and the slag discharge port are arranged on both sides of the short side of the slag furnace 3. The chute 2 is U-shaped, with an angle α of 75° with the vertical direction, a width B of 400 mm, a height H of 500 mm, and an internal melt depth of 80±10 mm; the discharge port 3-1 is trumpet-shaped, the length L1 of the discharge port 3-1 is 0.4 times the width of the slag furnace 3, the width L2 of the discharge port 3-1 is half the length L1, and the bottom surface of the discharge port 3-1 is inclined, and the angle β with the vertical direction is 45°. A feeding port 2-A with a diameter of 400 mm is provided at the top of the discharge port 3-1; two feeding ports 2-B1 and 2-B2 are provided at the top of the chute 2, which are distributed in sequence along the length direction, with a spacing of a=b=c, and the diameters of the feeding ports 2-B1 and 2-B2 are both 200 mm.

[0097] The hot lead smelting slag melt in the lead reduction furnace (reaction furnace 1) flows into the slag furnace through the chute 2, and the batch material in the front silo is quantitatively added from the charging port on the chute 2, spread on the surface of the hot lead smelting slag melt and enter the slag furnace together with the slag, and smelt for 100 minutes to obtain mineral wool melt and flue gas. The proportion of lead smelting slag and batch material is automatically controlled, that is, the slag discharge amount is pre-set according to 31 parts by weight of lead smelting slag melt, 48 parts by weight of batch material, and 36 parts by weight of garbage fly ash, and then the amount of batch material is calculated. After the batch material is weighed, a screw feeder is used to quantitatively add the material to the charging port on the chute, wherein 48 parts of batch material are added from the charging port 2-A, and 10 parts by weight, 12 parts by weight, and 14 parts by weight of garbage fly ash are added from the charging port 2-B1 and the charging port 2-B2, respectively.

[0098] The flue gas is firstly cooled to 200°C by a heat exchanger, and then the flue gas is purified to obtain flue dust. The flue dust contains 0.82% lead, and the lead recovery rate is 59.65%. The obtained flue dust is leached with soft water to obtain filtrate and filter residue, which is dried and ground to 200 mesh and added to the batch material in an amount of 1.0wt%; after the filtrate is concentrated, caustic alkali is added to precipitate lead, and crude salt is obtained by evaporation and crystallization.

[0099] The slag furnace maintains a stable melt of 1.8±0.1 times the single slag discharge amount of the lead reduction furnace, controls the temperature in the slag furnace to 1500±25℃, makes the viscosity of the mineral wool melt at the slag outlet to 0.4±0.1Pa·s, feeds the mineral wool melt into a four-roll centrifuge, and forms fibers to obtain cotton fibers with an average diameter of 5.4μm, wherein a composite binder such as phenolic resin, water repellent, and dustproof oil is applied during the fiber forming process. The leaching toxicity of the cotton fiber meets the limit value in the "Identification of Hazardous Waste Identification Standard Leaching Toxicity Identification" (GB 5085.3-2007).

[0100] The contents explained in the above embodiments should be understood as these embodiments are only used to more clearly illustrate the present invention, and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

Claims

1. A method for resource utilization of smelting slag, characterized in that: The steps include: S1. The smelting slag melt to be processed is fed into the slag furnace through a chute; at the same time, garbage fly ash and batch materials are added into the chute, so that the garbage fly ash and batch materials flow into the slag furnace together with the smelting slag melt, and are smelted to obtain mineral wool melt and flue gas; The ingredients of the batch material include one or more of CaO, MgO, SiO2, and Al2O3; the smelting slag is lead smelting slag; a plurality of feeding ports are arranged on the top of the chute, and the plurality of feeding ports are sequentially distributed along the length direction of the chute; along the flow direction of the smelting slag melt in the chute, garbage fly ash is added through the first 1-5 feeding ports, and the batch material is added through the last 1-3 feeding ports; the chute is a closed chute, and the top of the chute is connected to the flue of the slag furnace; the connection position between the chute and the slag furnace is higher than the liquid level in the slag furnace; S2, fiberizing the mineral wool melt to obtain cotton fibers; The flue gas is subjected to dust collection treatment to obtain smoke ash; and the smoke ash is then soaked in water to obtain filter residue and lead-containing filtrate.

2. The resource utilization method according to claim 1, characterized in that: The batch material comprises, by dry weight, 27-32 parts of fly ash, 12-18 parts of talcum powder, 0-8 parts of quartz powder and 0-2 parts of reducing agent.

3. The resource utilization method according to claim 2, characterized in that: In the lead smelting slag, the content of SiO2 is 25-30 wt%, the content of Al2O3 is 8-12 wt%, the content of Fe2O3 is 30-40 wt%, the content of CaO is 10-15 wt%, the content of MgO is 0-5 wt%, the sum of the contents of Na2O and K2O is ≤5 wt%, and the content of Pb is ≤2 wt%.

4. The resource utilization method according to claim 2, characterized in that: The garbage fly ash has a CaO content of 45-50 wt%, a chlorine content of 20-28 wt%, a Fe2O3 content of ≤5 wt%, and a total content of Na2O and K2O of ≤12 wt%; the fly ash component has a SiO2 content of 48-55 wt%, an Al2O3 content of 24-30 wt%, a Fe2O3 content of ≤6 wt%, and a total content of Na2O and K2O of ≤6 wt%; the talc powder has a SiO2 content of 48-54 wt%, and a MgO content of 25-30 wt%; and the quartz powder has a SiO2 content of ≥98 wt%.

5. The resource utilization method according to claim 1, characterized in that: The filter residue is returned to S1 and mixed into the batch material.

6. The resource utilization method according to claim 1, characterized in that: Calculated on a dry basis, the weight ratio of the lead smelting slag melt, the garbage fly ash and the batch material is 30-35:30-40:40-60.

7. The resource utilization method according to any one of claims 1 to 6, characterized in that: The multiple feeding ports are evenly distributed in sequence along the length direction of the chute.

8. The resource utilization method according to claim 7, characterized in that: The chute comprises a trough body, one end of which is provided with a feed port, and the other end of which is provided with a discharge port, which is connected to the slag furnace; the discharge port is trumpet-shaped, the bottom surface of the discharge port is inclined, and the angle β with the vertical direction is 20-50°.

9. The resource utilization method according to claim 8, characterized in that: The angle α between the tank body and the vertical direction is 70-85°.

10. The resource utilization method according to any one of claims 1 to 6, characterized in that: In S1, the melting time is 60-120 min.

11. The resource utilization method according to any one of claims 1 to 6, characterized in that: In S1, the batch material is evenly spread on the surface of the molten slag in the chute.