Bulletproof film for automobile

A bullet-proof film for automobiles is developed using polyurethaneimide and polyimide fiber layers, combined with polyphenylene ether and polycarbonate, addressing compatibility issues and enhancing thermal and mechanical properties for improved ballistic protection.

CN115847965BActive Publication Date: 2024-12-03DONGGUAN XIONGLIN NEW MATERIAL TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211305311.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-24
Publication Date
2024-12-03
Estimated Expiration
2042-10-24

AI Technical Summary

Technical Problem

Existing bulletproof materials often rely on ultra-high molecular weight polyethylene and aramid fiber which have a low melting point and poor compatibility, limiting their application in the bulletproof field.

Method used

A bullet-proof film for automobiles comprising a first bullet-proof film layer with polyurethaneimide and polyimide fiber, and a second bullet-proof film layer with polyphenylene ether, polycarbonate, and glass fiber, enhancing thermal properties, light transmittance, mechanical properties, and impact resistance.

Benefits of technology

The film achieves excellent thermal properties, high light transmittance, mechanical strength, and ballistic performance, with a thermal decomposition temperature above 420°C, glass transition temperature below -50°C, light transmittance above 91%, and impact resistance exceeding 46 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003905682020000031
    Figure BDA0003905682020000031
  • Figure BDA0003905682020000041
    Figure BDA0003905682020000041
  • Figure BDA0003905682020000071
    Figure BDA0003905682020000071
Patent Text Reader

Abstract

The present invention relates to a bulletproof film for automobiles, the bulletproof film for automobiles comprising a first bulletproof film layer and a second bulletproof film layer which are stacked; the first bulletproof film layer comprises the following components by weight: 60-80 parts of polyurethaneimide and 20-40 parts of polyimide fiber; the second bulletproof film layer comprises polyphenylene ether, polycarbonate, glass fiber and polyurethane. The bulletproof film for automobiles of the present invention has excellent thermal performance, light transmittance, mechanical properties, impact resistance and anti-ballistic performance, and has excellent comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bullet-proof films, in particular to a bullet-proof film for automobiles. Background Art

[0002] Currently, ultra-high molecular weight polyethylene and aramid fiber are mostly used in bulletproof materials. However, ultra-high molecular weight polyethylene has a low melting point and the two have poor compatibility, which limits its application in the bulletproof field.

[0003] CN107793700A discloses a composite material with a carbon fiber / polyimide fiber hybrid fabric as a reinforcing body and a preparation method thereof. The composite material disclosed therein is a hybrid fabric of carbon fiber and polyimide fiber obtained by blending or co-weaving the two, and then composited with corresponding resin and filler to prepare the composite material. The present invention adopts polyimide fiber as one of the main materials of the reinforcing body, and can well solve the brittleness problem of the composite material when only carbon fiber is used as the reinforcing body under the condition of not affecting the mechanical strength of the composite material, not only greatly improves its impact resistance, but also further improves the insulation performance of the composite material. The disclosed material can be applied to bulletproof vests, bulletproof bags, bulletproof armor, bulletproof shields, bulletproof helmets, safety helmets, crash walls, crash shields, bumpers, brake pads, grinding wheels, friction materials, and can also be used for the reinforcement, reinforcement and reinforcement of bridges and buildings.

[0004] CN108673984A discloses a bulletproof composite material, which is a resin-based composite material with polyimide fiber as a reinforcement, wherein the mass percentage of the polyimide fiber is 60% to 90%, and the mass percentage of the resin matrix is ​​10% to 40%. The polyimide fiber disclosed in the invention is a modified fiber that is subjected to interface treatment with an inert modifier, and the inert modifier is a mixture of water-based thermoplastic polyurethane and water-based polyolefin resin in a certain proportion. The invention also discloses a preparation method and application of the bulletproof composite material. The bulletproof composite material disclosed in the invention adopts polyimide fiber as a reinforcement, undergoes special interface treatment, is impregnated in a matrix resin in a certain arrangement mode, and is compounded with the matrix resin through a specific composite process. The prepared bulletproof composite material has high tensile strength and tensile modulus, good high and low temperature resistance, light weight, good flame retardancy and spinnability, and is suitable for preparing soft and comfortable bulletproof vests and bulletproof armor materials.

[0005] At present, although there are many studies on bulletproof materials, it is crucial to develop more bulletproof materials with excellent anti-ballistic properties. Summary of the invention

[0006] In view of the deficiencies of the prior art, the object of the present invention is to provide a bullet-proof film for automobiles, which has excellent thermal properties, light transmittance, mechanical properties, impact resistance and ballistic performance, and has excellent comprehensive performance.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a bullet-proof film for an automobile, the bullet-proof film for an automobile comprising a first bullet-proof film layer and a second bullet-proof film layer stacked;

[0009] The first bullet-proof film layer comprises the following components in parts by weight:

[0010] Polyurethaneimide 60-80 parts

[0011] 20-40 parts of polyimide fiber;

[0012] The second bullet-proof film layer comprises polyphenylene ether, polycarbonate, glass fiber and polyurethane.

[0013] In the present invention, the bulletproof film includes a double-layer structure, the first bulletproof film layer and the second bulletproof film layer cooperate with each other, wherein the polyimide fiber in the first bulletproof film layer forms the frame of the first bulletproof film layer, and then polyurethaneimide is arranged, the polyimide fiber ensures the bulletproof performance and heat resistance of the film layer, and the polyurethaneimide is used in conjunction with the second bulletproof film layer to enhance the interlayer force and ensure impact resistance; the second bulletproof film layer uses polyphenylene ether, polycarbonate, glass fiber and polyurethane to avoid excessive polyurethane reducing the mechanical properties of the system, and ensures the comprehensive performance of the formed automotive bulletproof film under the premise of less polyurethaneimide content. In addition, the bulletproof film described in the present invention has high light transmittance and low haze.

[0014] In the present invention, the weight proportion of the polyurethaneimide is 60-80 parts, for example, 62 parts, 64 parts, 66 parts, 68 parts, 70 parts, 72 parts, 74 parts, 76 parts, 78 parts, etc.

[0015] The weight proportion of the polyimide fiber is 20-40 parts, for example, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, etc.

[0016] Preferably, in the first bullet-proof film layer, the raw materials for preparing the polyurethaneimide include the following components in parts by weight:

[0017]

[0018] In the present invention, the weight proportion of the diisocyanate is 40-60 parts, for example, 42 parts, 44 parts, 46 parts, 48 ​​parts, 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, etc.

[0019] The weight proportion of the polyether polyol is 60-100 parts, for example, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts, etc.

[0020] The weight proportion of the chain extender is 10-20 parts, such as 12 parts, 14 parts, 16 parts, 18 parts, etc.

[0021] The weight portion of the catalyst is 0.01-1 part, for example, 0.05 part, 0.1 part, 0.2 part, 0.4 part, 0.6 part, 0.8 part, etc.

[0022] Preferably, the diisocyanate comprises any one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate or lysine diisocyanate, or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of toluene diisocyanate and isophorone diisocyanate, a combination of diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate and hexamethylene diisocyanate, a combination of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate, and the like.

[0023] Preferably, the polyether polyol comprises polyoxypropylene glycol and / or polytetramethylene glycol.

[0024] Preferably, the chain extender comprises an ether imide diol.

[0025] In the present invention, the chain extender is preferably ether imide diol, and the formed polyurethane imide has good compatibility with polyamide fiber and strong interaction with the second bullet-proof film layer, thereby ensuring the comprehensive performance of the bullet-proof film for automobiles.

[0026] Preferably, the catalyst comprises any one of organic bismuth, tetra-n-butyltin dibutyl or tin dilaurate, or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of organic bismuth and tetra-n-butyltin dibutyl, a combination of tetra-n-butyltin dibutyl and tin dilaurate, a combination of organic bismuth, tetra-n-butyltin dibutyl and tin dilaurate, and the like.

[0027] Preferably, the second bullet-proof film layer comprises the following components in parts by weight:

[0028]

[0029] In the present invention, the weight proportion of the polyphenylene ether is 30-50 parts, for example, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 ​​parts, etc.

[0030] The weight proportion of the polycarbonate is 20-50 parts, for example, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 45 parts, etc.

[0031] The weight proportion of the glass fiber is 3-5 parts, for example, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts, etc.

[0032] The weight proportion of the polyurethane is 3-10 parts, for example, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, etc.

[0033] Preferably, the mass ratio of the polyphenylene ether to the polycarbonate is (1-1.5):1, wherein 1-1.5 can be 1.1, 1.2, 1.3, 1.4, etc.

[0034] In the present invention, the polyphenylene ether and polycarbonate are used in a specific mass ratio, and the two act synergistically to ensure the compatibility of the components of the second bullet-proof film layer, thereby achieving heat resistance, impact resistance and bullet resistance.

[0035] Preferably, the thickness ratio of the first ballistic-proof film to the second ballistic-proof film is 1:(1-5), and 1-5 may be 1.5, 2, 2.5, 3, 3.5, 4, 4.5, etc.

[0036] In the present invention, the first bulletproof film and the second bulletproof film are used together at a specific thickness ratio so that the comprehensive performance of the automobile bulletproof film can be optimal. If the thickness of the first bulletproof film is too high, the amount of polyimide fiber used is too high, the cost is high and the performance improvement is limited; if the thickness of the second bulletproof film is too low, it is not enough to achieve excellent comprehensive performance.

[0037] In a second aspect, the present invention provides a bullet-proof film for automobile according to the first aspect, wherein a method for preparing the bullet-proof film for automobile comprises the following steps:

[0038] (1) weaving polyimide fibers and then impregnating them with polyurethaneimide to form a prepreg to obtain a first ballistic-proof film;

[0039] (2) Mixing polyphenylene ether, polycarbonate, glass fiber and polyurethane, melting them, extruding them onto the surface of the first bullet-proof film, and hot-pressing and curing them to form a second bullet-proof film, thereby obtaining the automobile bullet-proof film.

[0040] Preferably, in step (1), the method for preparing the polyurethaneimide comprises the following steps:

[0041] The diisocyanate, polyether polyol and catalyst are mixed, prepolymerized, and then mixed with a chain extender and polymerized to obtain the polyurethaneimide.

[0042] Preferably, the prepolymerization temperature is 50-100°C, such as 55°C, 60°C, 70°C, 80°C, 90°C, etc.

[0043] Preferably, the prepolymerization time is 2-4 h, such as 2.5 h, 3 h, 3.5 h, 4 h, etc.

[0044] Preferably, the polymerization temperature is 110-160°C, for example, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, etc.

[0045] Preferably, the polymerization time is 3-8 h, for example, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h, etc.

[0046] Preferably, in step (2), the temperature of the hot pressing curing is 100-500°C, for example, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, etc.

[0047] Preferably, the pressure of the hot pressing curing is ≥0.2 MPa, such as 0.3 MPa, 0.5 MPa, 1 MPa, 1.5 MPa, etc.

[0048] Preferably, the hot pressing curing time is 0.5-2 h, for example, 0.6 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, etc.

[0049] As a preferred technical solution, the preparation method comprises the following steps:

[0050] (1) mixing a diisocyanate, a polyether polyol and a catalyst, prepolymerizing at 50-100° C. for 2-4 hours, and then mixing with a chain extender, polymerizing at 110-160° C. for 3-8 hours to obtain the polyurethaneimide;

[0051] The polyimide fibers are braided and then impregnated with polyurethaneimide to form a prepreg to obtain a first bullet-proof film;

[0052] (2) polyphenylene ether, polycarbonate, glass fiber and polyurethane are mixed, melted, extruded onto the surface of the first bullet-proof film, and hot-pressed and cured at ≥0.2 MPa and 100-500° C. for 0.5-2 h to form a second bullet-proof film, thereby obtaining the automotive bullet-proof film.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The automotive bullet-proof film of the present invention has excellent thermal properties, light transmittance, mechanical properties, impact resistance and ballistic resistance, and has excellent comprehensive performance.

[0055] (2) The thermal decomposition temperature of 5 wt% of the automotive bullet-proof film of the present invention is above 420°C, the glass transition temperature is less than -50°C, the light transmittance is above 91%, the haze is above 0.5%, the bending strength is above 568 MPa, the number of impact resistance is above 46 times, the tensile strength is above 53.8 MPa, the tear strength is above 35.1 KN / M, the elongation at break is above 542%, the bonding strength with polycarbonate is above 13.2 KN / M, and the bullet-proof performance meets the standard requirements. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] Example 1

[0058] The present embodiment provides a bullet-proof film for automobiles, the bullet-proof film for automobiles comprising a first bullet-proof film layer and a second bullet-proof film layer stacked in a thickness ratio of 1:3;

[0059] The first bullet-proof film layer comprises the following components in parts by weight:

[0060] Polyurethaneimide 70 parts

[0061] 30 parts of polyimide fiber;

[0062] Wherein, the raw materials for preparing the polyurethaneimide include the following components:

[0063]

[0064] The second bullet-proof film layer comprises the following components in parts by weight:

[0065]

[0066] In this embodiment, the polyimide fiber is purchased from Forsman Technology Co., Ltd.; the diisocyanate is toluene diisocyanate; the polyether polyol is polyoxypropylene glycol, purchased from Wuhan Fuxinyuan Technology Co., Ltd.; the chain extender is methoxy polyethylene glycol maleimide, purchased from Beijing Jiankai Technology Co., Ltd.; the catalyst is organic bismuth, purchased from Shanghai Koraman Reagent Co., Ltd., with a brand number of 093411; polyphenylene ether is purchased from Shanghai Koraman Reagent Co., Ltd., with a brand number of 160649; and polycarbonate is purchased from Shanghai Yien Chemical Technology Co., Ltd., with a brand number of R0055043.

[0067] The automotive bulletproof film is prepared by the following method, which comprises the following steps:

[0068] (1) mixing a diisocyanate, a polyether polyol and a catalyst, heating them to 50° C., 60° C., 80° C. and 100° C. in sequence, reacting them for 0.5 h each, then mixing them with a chain extender, polymerizing them at 110° C., 120° C., 130° C. and 140° C. for 2 h each, to obtain the polyurethaneimide;

[0069] The polyimide fibers are braided and then impregnated with polyurethaneimide to form a prepreg to obtain a first bullet-proof film;

[0070] (2) mixing polyphenylene ether, polycarbonate, glass fiber and polyurethane, melting them, extruding them onto the surface of the first bullet-proof film, and hot-pressing and curing them at 2 MPa and 300° C. for 1.5 h to form a second bullet-proof film, thereby obtaining the automotive bullet-proof film;

[0071] The polyurethane is prepared by replacing the chain extender in step (1) with an equal mass of ethylenediamine.

[0072] Example 2

[0073] The present embodiment provides a bullet-proof film for automobiles, the bullet-proof film for automobiles comprising a first bullet-proof film layer and a second bullet-proof film layer stacked in a thickness ratio of 1:5;

[0074] The first bullet-proof film layer comprises the following components in parts by weight:

[0075] Polyurethaneimide 80 parts

[0076] 20 parts of polyimide fiber;

[0077] Wherein, the raw materials for preparing the polyurethaneimide include the following components:

[0078]

[0079]

[0080] The second bullet-proof film layer comprises the following components in parts by weight:

[0081]

[0082] In this embodiment, the polyimide fiber is purchased from Forsman Technology Co., Ltd.; the diisocyanate is diphenylmethane diisocyanate and dicyclohexylmethane diisocyanate of equal mass; the polyether polyol is polyoxypropylene glycol, purchased from Wuhan Fuxinyuan Technology Co., Ltd.; the chain extender is methoxy polyethylene glycol maleimide, purchased from Beijing Jiankai Technology Co., Ltd.; the catalyst is tetra-n-butyltin dibutyl; polyphenylene ether is purchased from Shanghai Koraman Reagent Co., Ltd. with a brand name of 160649; and polycarbonate is purchased from Shanghai Yien Chemical Technology Co., Ltd. with a brand name of R0055043.

[0083] The automotive bulletproof film is prepared by the following method, which comprises the following steps:

[0084] (1) mixing a diisocyanate, a polyether polyol and a catalyst, heating to 50° C., 60° C., 70° C. and 80° C. for reaction for 0.5 h, 1 h, 2 h and 0.5 h, respectively, and then mixing with a chain extender, polymerizing at 110° C., 120° C., 130° C. and 150° C. for 1 h respectively to obtain the polyurethaneimide;

[0085] The polyimide fibers are braided and then impregnated with polyurethaneimide to form a prepreg to obtain a first bullet-proof film;

[0086] (2) polyphenylene ether, polycarbonate, glass fiber and polyurethane are mixed, melted, extruded onto the surface of the first bullet-proof film, and hot-pressed and cured at 0.2 MPa and 500° C. for 0.5 h to form a second bullet-proof film, thereby obtaining the automobile bullet-proof film.

[0087] Example 3

[0088] The present embodiment provides a bullet-proof film for automobiles, the bullet-proof film for automobiles comprising a first bullet-proof film layer and a second bullet-proof film layer stacked in a thickness ratio of 1:1;

[0089] The first bullet-proof film layer comprises the following components in parts by weight:

[0090] Polyurethaneimide 60 parts

[0091] 40 parts of polyimide fiber;

[0092] Wherein, the raw materials for preparing the polyurethaneimide include the following components:

[0093]

[0094] The second bullet-proof film layer comprises the following components in parts by weight:

[0095]

[0096] In this embodiment, the polyimide fiber is purchased from Forsman Technology Co., Ltd.; the diisocyanate is hexamethylene diisocyanate; the polyether polyol is polytetramethylene glycol, purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; the chain extender is methoxy polyethylene glycol maleimide, purchased from Beijing Jiankai Technology Co., Ltd.; the catalyst is tin dilaurate; polyphenylene ether is purchased from Shanghai Koraman Reagent Co., Ltd. with a brand number of 160649; and polycarbonate is purchased from Shanghai Eon Chemical Technology Co., Ltd. with a brand number of R0055043.

[0097] The automotive bulletproof film is prepared by the following method, which comprises the following steps:

[0098] (1) mixing a diisocyanate, a polyether polyol and a catalyst, heating to 50° C., 60° C., 70° C. and 80° C. for reaction for 0.5 h, 1 h, 2 h and 0.5 h, respectively, and then mixing with a chain extender, polymerizing at 110° C., 120° C., 130° C. and 150° C. for 1 h respectively to obtain the polyurethaneimide;

[0099] The polyimide fibers are braided and then impregnated with polyurethaneimide to form a prepreg to obtain a first bullet-proof film;

[0100] (2) polyphenylene ether, polycarbonate, glass fiber and polyurethane are mixed, melted, extruded onto the surface of the first bullet-proof film, and hot-pressed and cured at 3 MPa and 160° C. for 2 h to form a second bullet-proof film, thereby obtaining the automotive bullet-proof film.

[0101] Example 4

[0102] The difference between this embodiment and embodiment 1 is that the ether imide diol is replaced by ethylenediamine of equal mass, and 8 parts of trimellitic anhydride are added in the process of preparing polyurethaneimide, and the rest is the same as embodiment 1.

[0103] Embodiment 5-6

[0104] The difference between Example 5-6 and Example 1 is that the mass of polyphenylene ether remains unchanged, the mass ratio of polyphenylene ether to polycarbonate is 2:1 (Example 5) and 0.8:1 (Example 6), and the rest is the same as Example 1.

[0105] Embodiment 7-8

[0106] The difference between Example 7-8 and Example 1 is that the thickness ratios of the first ballistic-proof film and the second ballistic-proof film are 1:0.5 (Example 7) and 1:5.5 (Example 8), respectively, and the rest are the same as Example 1.

[0107] Comparative Example 1

[0108] The difference between this comparative example and Example 1 is that the polyurethaneimide is replaced by an equal mass of polyurethane, and the difference between the preparation raw materials of the polyurethane and the polyurethaneimide in Example 1 is that the chain extender is replaced by an equal mass of ethylenediamine, and the rest is the same as Example 1.

[0109] Comparative Example 2

[0110] The difference between this comparative example and Example 1 is that the polycarbonate is replaced by polyphenylene ether of equal mass, and the rest is the same as Example 1.

[0111] Comparative Example 3

[0112] The difference between this comparative example and Example 1 is that the polyphenylene ether is replaced by polycarbonate of equal mass, and the rest is the same as Example 1.

[0113] Performance Testing

[0114] The automotive bullet-proof films described in Examples 1-8 and Comparative Examples 1-3 were tested as follows:

[0115] (1) Thermal decomposition temperature: The thermal decomposition temperature of 5 wt% was calculated by heating at a rate of 10 °C / min using a thermogravimetric analyzer;

[0116] Glass transition temperature (T g , ℃): tested by differential scanning calorimeter.

[0117] (2) Flexural strength: tested in accordance with ASTM D6415 / D6415M-06a (2013).

[0118] (3) Impact resistance: The test was conducted using a heavy hammer impact method. The single impact energy was 2.5 J and the average number of impacts on the test sample was 2.5 J.

[0119] (4) Ballistic performance: Tested in accordance with NIJ Standard-0101.04, V50 performance is recorded, and the deformation values ​​displayed are divided into Level 1, Level 2, Level 3 and Level 4 from low to high;

[0120] (5) Light transmittance and haze: tested in accordance with GB / T2410-2008;

[0121] (6) Tensile strength, tear strength and elongation at break: tested in accordance with GB / T528-2008;

[0122] (7) Bonding strength with PC (polycarbonate): Tested in accordance with Q / 6S 2767-2013.

[0123] The test results are summarized in Tables 1 and 2.

[0124] Table 1

[0125]

[0126]

[0127] Table 2

[0128]

[0129]

[0130] Analysis of the data in Table 1 and Table 2 shows that the thermal decomposition temperature of 5wt% of the bullet-proof film for automobiles of the present invention is above 420°C, the glass transition temperature is less than -50°C, the light transmittance is above 91%, the haze is above 0.5%, the bending strength is above 568MPa, the number of impact resistance is above 46 times, the tensile strength is above 53.8MPa, the tear strength is above 35.1KN / M, the elongation at break is above 542%, the bonding strength with polycarbonate is above 13.2KN / M, and the bulletproof performance meets the standard requirements; the bullet-proof film for automobiles of the present invention has excellent thermal properties, light transmittance, mechanical properties, impact resistance and bulletproof performance, and has excellent comprehensive performance.

[0131] Analysis of Comparative Example 1 and Example 1 shows that the performance of Comparative Example 1 is not as good as that of Example 1, which proves that the automotive bullet-proof film formed by setting polyurethaneimide in the first bullet-proof film of the present invention has better performance.

[0132] Analysis of Comparative Examples 2-3 and Example 1 shows that the performance of Comparative Examples 2-3 is not as good as that of Example 1, which proves that the automotive bullet-proof film formed by the combination of polyphenylene ether and polycarbonate in the first bullet-proof film of the present invention has better performance.

[0133] Analysis of Example 4 and Example 1 shows that the performance of Example 4 is not as good as that of Example 1, which proves that the performance of the automotive bullet-proof film formed by the direct polymerization of polyurethane and polyimide is worse than that of the polyurethane imide using ether imide diol chain extender.

[0134] Analysis of Examples 5-6 and Example 1 shows that the performance of Examples 5-6 is not as good as that of Example 1, which proves that in the present invention, the automotive bullet-proof film formed when the mass ratio of the polyphenylene ether to the polycarbonate is in the range of (1-1.5):1 has better performance.

[0135] Analysis of Examples 7-8 and Example 1 shows that the performance of Examples 7-8 is not as good as that of Example 1, which proves that in the present invention, the automotive bullet-proof film formed when the thickness ratio of the first bullet-proof film to the second bullet-proof film is within the range of 1:(1-5) has better performance.

[0136] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A bullet-proof film for automobiles, characterized in that: The automotive bulletproof film comprises a first bulletproof film layer and a second bulletproof film layer which are stacked; The first bullet-proof film layer comprises the following components in parts by weight: Polyurethaneimide 60-80 parts 20-40 parts of polyimide fiber; In the first bullet-proof film layer, the raw materials for preparing the polyurethaneimide include the following components in parts by weight: The chain extender includes ether imide diol; The second bullet-proof film layer comprises the following components in parts by weight: The mass ratio of the polyphenylene ether to the polycarbonate is (1-1.5):

1.

2. The bullet-proof film for automobile according to claim 1, characterized in that: The diisocyanate includes any one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate or lysine diisocyanate, or a combination of at least two thereof.

3. The bullet-proof film for automobile according to claim 1, characterized in that: The polyether polyol includes polyoxypropylene glycol and / or polytetramethylene glycol.

4. The bullet-proof film for automobile according to claim 1, characterized in that: The catalyst includes any one of organic bismuth, dibutyl tetra-n-butyltin or tin dilaurate, or a combination of at least two thereof.

5. The bullet-proof film for automobile according to claim 1, characterized in that: The thickness ratio of the first ballistic-proof film to the second ballistic-proof film is 1:(1-5).

6. The bullet-proof film for automobile according to any one of claims 1 to 5, characterized in that: The method for preparing the automotive bulletproof film comprises the following steps: (1) weaving polyimide fibers and then impregnating them with polyurethaneimide to form a prepreg to obtain a first ballistic-proof film; (2) Mixing polyphenylene ether, polycarbonate, glass fiber and polyurethane, melting them, extruding them onto the surface of the first bullet-proof film, and hot-pressing and curing them to form a second bullet-proof film, thereby obtaining the automobile bullet-proof film.

7. The bullet-proof film for automobile according to claim 6, characterized in that: In step (1), the preparation method of the polyurethaneimide comprises the following steps: The diisocyanate, polyether polyol and catalyst are mixed, prepolymerized, and then mixed with a chain extender and polymerized to obtain the polyurethaneimide.

8. The bullet-proof film for automobile according to claim 7, characterized in that: The prepolymerization temperature is 50-100°C.

9. The bullet-proof film for automobile according to claim 7, characterized in that: The prepolymerization time is 2-4 hours.

10. The bullet-proof film for automobile according to claim 7, characterized in that: The polymerization temperature is 110-160°C.

11. The bullet-proof film for automobile according to claim 7, characterized in that: The polymerization time is 3-8h.

12. The bullet-proof film for automobile according to claim 6, characterized in that: In step (2), the temperature of the hot pressing curing is 100-500°C.

13. The bullet-proof film for automobile according to claim 6, characterized in that: The pressure of the hot pressing curing is ≥0.2MPa.

14. The bullet-proof film for automobile according to claim 6, characterized in that: The time of the hot pressing curing is 0.5-2h.

15. The bullet-proof film for automobile according to claim 6, characterized in that: The preparation method comprises the following steps: (1) mixing a diisocyanate, a polyether polyol and a catalyst, prepolymerizing at 50-100° C. for 2-4 hours, and then mixing with a chain extender, polymerizing at 110-160° C. for 3-8 hours to obtain the polyurethaneimide; The polyimide fibers are braided and then impregnated with polyurethaneimide to form a prepreg to obtain a first bullet-proof film; (2) polyphenylene ether, polycarbonate, glass fiber and polyurethane are mixed, melted, extruded onto the surface of the first bullet-proof film, and hot-pressed and cured at ≥0.2 MPa and 100-500° C. for 0.5-2 h to form a second bullet-proof film, thereby obtaining the automotive bullet-proof film.

Citation Information

Patent Citations

  • Composite material taking carbon fiber / polyimide fiber hybrid fabric as enhancing body and preparation method thereof

    CN107793700A

  • Polyurethane-imide-base multifunctional composite damping material and preparation method thereof

    CN104877336A

  • Bulletproof composite material and preparation method and application thereof

    CN108673984A