A bending-resistant insulating epoxy composite heat dissipation film for solar energy and its production process
By using a bending-resistant insulated epoxy composite film on solar cells, using the combination of refracting plate sheets and crystal polypyramid structures, the problems of high cost and saturated heat dissipation performance of traditional cooling methods are solved, and more efficient thermal radiation and visible light are achieved Management improves the efficiency and life of solar cells.
Patent Information
- Application Number
- CN202211488065.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-25
AI Technical Summary
The traditional cooling method of existing solar cells is high in cost and low in reliability, and the high temperature limits the solar photoelectric conversion efficiency. The existing heat dissipation film cannot further extend after the temperature reaches saturation.
A bending-resistant insulated epoxy composite heat dissipation film is used to reflect the infrared light source back into the atmosphere through the secondary reflection of the refractive plate sheet, and a crystal polypyramid structure is used to reduce the light transmission effect of visible light and improve radiation performance.
It effectively reduces the surface temperature of the solar cell, suppresses the temperature increase, improves radiation performance, ensures the transmittance of visible light, and extends the service life of the film.
Smart Images

Figure CN115847982B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar heat dissipation, in particular to a bending-resistant insulating epoxy composite heat dissipation film for solar energy and a production process thereof. Background Art
[0002] Solar photovoltaic conversion is the most common way to utilize solar energy, and solar cells are the core components of solar photovoltaic conversion. Due to the low conversion efficiency of solar cells, most of the absorbed solar radiation is dissipated as heat energy, which increases the temperature of the battery. Excessive temperature further limits the conversion efficiency of solar cells. Therefore, lowering the operating temperature is crucial for solar photovoltaic conversion. The traditional cooling method for solar cells is mainly active cooling, which requires additional energy-consuming equipment, is costly, complex to install, and has low reliability.
[0003] A Chinese patent with publication number CN109206863A discloses a method for preparing an anti-corrosion and highly transparent heat-dissipating film for solar panels. The process is simple and the operation is convenient. The prepared anti-corrosion and highly transparent heat-dissipating film not only has a good heat dissipation effect, but also has excellent corrosion resistance, aging resistance, and high transmittance. The film has excellent mechanical properties, which greatly extends the service life of the film.
[0004] In the above patent, the high thermal conductivity of graphene material is used to achieve rapid heat dissipation for solar energy, but the heat dissipation process of the material itself is a cycle of absorption and transfer, and its efficient heat dissipation performance is based on the thermal conductivity of the material itself and the temperature of the surrounding environment. Once the material and the ambient temperature reach saturation, the heat dissipation cannot be further extended, and the film structure will be in a high-temperature environment; therefore, it does not meet the existing needs, and a bend-resistant insulating epoxy composite heat dissipation film for solar energy and its production process are proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a bending-resistant insulating epoxy composite heat dissipation film for solar energy and its production process, which has the function of reflecting the infrared light source with thermal radiation back into the atmosphere through secondary reflection of the refractive plate, and the actual refractive index will slowly change from the tip to the bottom of the pyramid, which helps to reduce reflection and improve radiation performance. The refractive plate also has a function of refracting the crystal itself and reflecting the visible light source after multiple refractions to irradiate the photovoltaic panel, thereby reducing the influence of the crystal structure on the transmittance of visible light, ensuring the transmittance of visible light, and solving the problems in the prior art.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a bending-resistant insulating epoxy composite heat dissipation film for solar energy, comprising an epoxy composite film body, wherein the epoxy composite film body comprises an epoxy resin surface film, an epoxy resin bottom film, a crystalline silicon radiation layer and a convection grid pad layer, wherein the convection grid pad layer is arranged above the epoxy resin bottom film, the crystalline silicon radiation layer is arranged above the convection grid pad layer, and the epoxy resin surface film is arranged above the crystalline silicon radiation layer.
[0007] Preferably, the crystalline silicon radiation layer includes a crystal polygonal pyramid, and the crystal polygonal pyramid includes an incident plate and a refraction plate. The refraction plate is arranged above the incident plate, and there are four refraction plates.
[0008] Preferably, the convection grille cushion layer comprises a thermal insulation rubber net, and heat dissipation convection grooves are arranged between the thermal insulation rubber nets.
[0009] Preferably, the outer surface of the epoxy resin surface film is provided with a thermal conductive coating, and the outer surface of the epoxy resin base film is provided with a thermal conductive grease.
[0010] A production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy, comprising the following steps:
[0011] Step 1: Pour the selected epoxy resin particles into an ultrasonic cleaning machine for cleaning to remove excess dust on the surface. After cleaning, put the resin particles into a dryer to remove residual moisture on the surface. The drying temperature is about 150-160°C and the drying time is about 3-4 hours.
[0012] Step 2: Add the dried resin particles together with the additives into the blow molding machine for heating at a temperature of 320-450°C. After the raw materials are melted, they are stirred by the stirring structure inside the blow molding machine at a speed of 600-800r / min.
[0013] Step 3: After stirring evenly, the liquid raw material is extruded into shape by an extruder, the temperature of the extruder head is 210-280°C, and the extruded raw material is stretched and then formed into an epoxy resin surface film and an epoxy resin bottom film in two steps, wherein the thickness of the epoxy resin surface film is less than that of the epoxy resin bottom film;
[0014] Step 4: Mix the silicon source containing silicon dioxide, water, structure directing agent and alkali in a certain proportion, put them into a pressure-resistant reactor and seal them, then heat them to 100-220°C and keep the temperature constant for 5-10 hours. After the reaction is completed, cool the reactor quickly;
[0015] Step 5: Wash the reaction product with water until the pH is 8-11, and dry the reaction product to obtain raw powder, pour the raw powder into a special mold, and then put the mold and the raw powder into a tube furnace for roasting and activation. After sintering and forming, naturally cool to room temperature to obtain a crystalline polygonal pyramid;
[0016] Step 6: Cover one side of the epoxy resin base film with a convection grille cushion layer, which is made of a high-transmittance soft rubber material, and then lay a crystal polygonal pyramid on the top of the convection grille cushion layer, with the cone corresponding to the position of the convection mesh surface groove;
[0017] Step 7: After the laying is completed, put the epoxy resin base film and the crystal polygonal pyramid into the mold frame, inject the adhesive liquid into the surface of the crystal polygonal pyramid, the glue filling height is consistent with the cone height, and finally cover the epoxy resin surface film on the top of the crystal polygonal pyramid;
[0018] Step 8: Use a hot pressing plate to perform hot pressing on the entire composite membrane structure to allow the glue to melt and infiltrate the membrane structure. After the hot pressing is completed, the composite membrane is taken out and cooled naturally. At this time, the internal crystal polygonal pyramid can form a group of crystalline silicon radiation layers after being filled with glue and cooled.
[0019] Preferably, in step three, in the process of preparing the epoxy resin base film, silver powder needs to be added to the raw material, and the ratio of silver powder to raw material is 1:50, wherein the particle size of the silver powder is 0.5-0.7 μm, and its shape is flaky or polygonal structure.
[0020] Preferably, in step five, the diameter of the crystal polygonal pyramid is 250 μm and the height is 250 μm.
[0021] Preferably, in step six, when laying the crystal polygonal pyramid structure, a filling gap needs to be reserved between the crystal polygonal pyramids, and the width of the filling gap is 0.1 mm.
[0022] Preferably, in step seven, after the laying of the crystal polygonal pyramid is completed, the excess part of the base film needs to be cut off, and then the edge wrapping operation is performed after the cutting, and the raw material structure required for the edge wrapping is consistent with the base film.
[0023] Preferably, in step eight, the thickness of the composite film is 280-290 μm.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] In the present invention, the main raw material of the crystal polygonal pyramid is silicon dioxide. Silicon dioxide itself has an extremely high transmittance to visible light, but a relatively low transmittance to infrared light with a wavelength above 4μm. The crystal polygonal pyramid is laid between the epoxy film. When sunlight shines on the incident film surface of the crystal polygonal pyramid through the film surface, the visible light can directly pass through the incident film and continue to extend downward to the surface of the photovoltaic panel, and the infrared light will be reflected when it contacts the incident film. The reflected light will shine on the refraction plates on both sides, and finally, through the secondary reflection of the refraction plates, the infrared light source with thermal radiation is reflected back into the atmosphere, and the actual refractive index will slowly change from the tip to the bottom of the pyramid, which is helpful to reduce reflection and improve radiation performance. The refraction plates also have another function of refracting the visible light source refracted by the crystal itself and reflected onto the photovoltaic panel after multiple refractions, thereby reducing the influence of the crystal structure on the transmittance of visible light and ensuring the transmittance of visible light. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the overall front view of the present invention;
[0027] Figure 2 It is a schematic diagram of the overall side section structure of the present invention;
[0028] Figure 3 It is a schematic diagram of the structure of the crystalline silicon radiation layer of the present invention;
[0029] Figure 4 It is a schematic diagram of the structure of the convection grid cushion layer of the present invention;
[0030] Figure 5 It is a schematic diagram of the crystal polygonal pyramid structure of the present invention;
[0031] Figure 6 It is a schematic diagram of the crystal polygonal pyramid heat radiation reflection structure of the present invention.
[0032] In the figure: 1. epoxy composite film body; 101. epoxy resin surface film; 102. epoxy resin bottom film; 103. crystalline silicon radiation layer; 104. convection grid cushion layer; 1031. crystal polygonal pyramid; 1032. incident film; 1033. refraction plate; 1041. thermal insulation glue net; 1042. convection grid surface groove. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] See also Figure 1-2 An embodiment of the present invention is as follows: a bending-resistant insulating epoxy composite heat dissipation film for solar energy, comprising an epoxy composite film body 1, wherein the epoxy composite film body 1 comprises an epoxy resin surface film 101, an epoxy resin bottom film 102, a crystalline silicon radiation layer 103 and a convection grid pad 104, wherein the convection grid pad 104 is arranged above the epoxy resin bottom film 102, the crystalline silicon radiation layer 103 is arranged above the convection grid pad 104, and the epoxy resin surface film 101 is arranged above the crystalline silicon radiation layer 103.
[0035] See also Figure 3-6 The crystalline silicon radiation layer 103 includes a crystal polygonal pyramid 1031, and the crystal polygonal pyramid 1031 includes an incident bottom plate 1032 and a refraction plate 1033, and the refraction plate 1033 is arranged above the incident bottom plate 1032, and there are four refraction plates 1033. The convection grid pad 104 includes a heat-insulating glue net 1041, and heat-dissipating convection grooves are arranged between the heat-insulating glue nets 1041. The outer surface of the epoxy resin surface film 101 is provided with a thermal conductive coating, and the outer surface of the epoxy resin bottom film 102 is provided with a thermal conductive grease;
[0036] The main raw material of the crystal polygonal pyramid 1031 is silicon dioxide. Silicon dioxide itself has a very high transmittance to visible light, but its transmittance to infrared light with a wavelength of more than 4μm is relatively low. The crystal polygonal pyramid 1031 is laid between the epoxy film. When sunlight shines on the incident film 1032 surface of the crystal polygonal pyramid 1031 through the film surface, the visible light can directly pass through the incident film 1032 and continue to extend downward to the surface of the photovoltaic panel. When the infrared light contacts the incident film 1032, it will be reflected. The reflected light will shine on the refraction plates 1033 on both sides. Finally, through the secondary reflection of the refraction plates 1033, the infrared light source with thermal radiation is reflected back into the atmosphere. From the tip to the bottom of the pyramid, the actual refractive index will slowly change, which helps to reduce reflection and improve radiation performance. The refraction plate 1033 also has another function, which is to refract the visible light source refracted by the crystal itself and reflected by it after multiple refractions and shine it on the photovoltaic panel, thereby reducing the influence of the crystal structure on the transmittance of visible light and ensuring the transmittance of visible light.
[0037] After the experiment, at 800W / m 2 The temperature rise under sunlight is suppressed to 19.7K, the surface temperature of the solar cell is only about 49.7℃, and the output power only drops by about 8%.
[0038] A production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy, comprising the following steps:
[0039] Step 1: Pour the selected epoxy resin particles into an ultrasonic cleaning machine for cleaning to remove excess dust on the surface. After cleaning, put the resin particles into a dryer to remove residual moisture on the surface. The drying temperature is about 150-160°C and the drying time is about 3-4 hours.
[0040] Step 2: Add the dried resin particles together with the additives into the blow molding machine for heating at a temperature of 320-450°C. After the raw materials are melted, they are stirred by the stirring structure inside the blow molding machine at a speed of 600-800r / min.
[0041] Step 3: After stirring evenly, the liquid raw material is extruded into shape by an extruder, the temperature of the extruder head is 210-280°C, and the extruded raw material is stretched and then formed into an epoxy resin surface film 101 and an epoxy resin base film 102 in two steps, wherein the thickness of the epoxy resin surface film 101 is less than that of the epoxy resin base film 102. In the process of preparing the epoxy resin base film 102, silver powder needs to be added to the raw material, and the ratio of the silver powder to the raw material is 1:50, wherein the particle size of the silver powder is 0.5-0.7 μm, and its shape is a sheet or polygonal structure;
[0042] Step 4: Mix the silicon source containing silicon dioxide, water, structure directing agent and alkali in a certain proportion, put them into a pressure-resistant reactor and seal them, then heat them to 100-220°C and keep the temperature constant for 5-10 hours. After the reaction is completed, cool the reactor quickly;
[0043] Step 5: washing the reaction product with water until the pH value is 8-11, and drying the reaction product to obtain raw powder, pouring the raw powder into a special mold, and then putting the mold and the raw powder into a tube furnace for roasting and activation, and naturally cooling to room temperature after sintering, thereby obtaining a crystal polygonal pyramid 1031, the diameter of the crystal polygonal pyramid 1031 is 250 μm, and the height is 250 μm;
[0044] Step 6: Cover one side of the epoxy resin base film 102 with a convection grid cushion layer 104, which is made of a high-transmittance soft rubber material, and then lay the crystal polygonal pyramid 1031 on the convection grid cushion layer 104, with the position of the cone corresponding to the convection mesh surface groove 1042. When laying the crystal polygonal pyramid 1031 structure, a filling gap needs to be reserved between the crystal polygonal pyramids 1031, and the width of the filling gap is 0.1 mm;
[0045] Step 7: After the laying is completed, the epoxy resin base film 102 and the crystal polygonal pyramid 1031 are placed in the mold frame, and the adhesive liquid is injected into the surface of the crystal polygonal pyramid 1031. The height of the adhesive liquid filling is consistent with the height of the cone. Finally, the epoxy resin surface film 101 is covered on the top of the crystal polygonal pyramid 1031. After the laying of the crystal polygonal pyramid 1031 is completed, the excess part of the base film needs to be cut off, and the edge wrapping operation is performed after the cutting. The raw material structure required for the edge wrapping is consistent with the base film;
[0046] Step 8: Use a hot pressing plate to perform hot pressing on the entire composite membrane structure to allow the glue to melt and infiltrate the membrane structure. After the hot pressing is completed, the composite membrane is taken out and cooled naturally. At this time, the internal crystal polygonal pyramid 1031 can form a group of crystalline silicon radiation layers 103 after being filled with glue and cooled. The thickness of the composite membrane is 280-290μm.
[0047] The energy balance of solar cells mainly involves four types of energy: the heating power q of solar radiation, the thermal radiation power P of the solar cell itself, and the rad (T cell ), where T cell is the temperature of the solar cell, in K, and the thermal radiation P absorbed by the solar cell from the atmosphere atm (T a ), where T a is the ambient temperature, in K, and the convection / conduction heat dissipation power P between the solar cell and the ambient air con (T cell , T a ), according to the first law of thermodynamics, the energy control equation of the solar cell can be obtained, and the specific expression is:
[0048]
[0049] The thermal radiation power P of the solar cell itself rad (T cell ) is related to the battery temperature and emissivity spectrum, and its expression is as follows:
[0050]
[0051] Where Ω is the radiation solid angle; I BB (T cell , λ) is the temperature T cell The blackbody spectral radiation power; ε(λ, Ω) is the spectral directional emissivity of the solar cell; According to the definition of solid angle and Planck's law, the differential of the radiation solid angle dΩ and T cell The blackbody spectral radiation power at temperature is expressed as:
[0052]
[0053]
[0054] In the formula, h is Planck's constant, which is 6.626×10-34J·s; c is the speed of light, which is 2.998x 10ms -1 ; λ is the wavelength, k B is the Boltzmann constant, which is 1.381×10-23K -1 ;
[0055] The thermal radiation P absorbed by the solar cell from the atmosphere atm (T a ) is mainly related to the ambient temperature and the battery absorptivity (emissivity) spectrum. The specific expression is as follows:
[0056]
[0057] In the formula, I BB (T a , λ) is the temperature T a The blackbody spectral radiation power; α(λ, Ω) is the spectral directional absorption rate of the solar cell. According to Kirchhoff's law, α(λ, Ω) = ε(λ, Ω); ε atm (λ, Ω) is the spectral directional emissivity of the atmosphere. Since the radiation characteristics of the atmosphere are relatively complex, empirical or semi-empirical formulas are often used to describe atmospheric radiation. In the field of radiation cooling, ε atm (λ, Ω) can be described by the following expression:
[0058] ε aim (λ,Ω)=1-t(λ) 1 / cosθ (2-6)
[0059] Where t(λ) is the spectral transmittance of the atmosphere in the vertical direction, which is closely related to the parameters of the atmosphere, such as atmospheric water content, aerogel conditions, and cloud coverage;
[0060] Convection / heat dissipation power P between solar cells and ambient air con (T cell , T a ) is related to the battery temperature, ambient temperature and the heat transfer coefficient between the two. When there is a difference between the temperature of the solar cell and the ambient temperature, the influence of the temperature gradient makes convection and heat conduction between the two inevitable, and its intensity can be evaluated by the heat transfer coefficient between the two. The specific expression is as follows:
[0061] P con (T cell , T a )=h c (T cell -Ta ) ( 2-7)
[0062] In the formula, h c It is the total heat transfer coefficient of thermal conductivity / convection between solar cells and ambient air, which is closely related to parameters such as wind speed, ambient temperature, and device structure.
[0063] In the integral process related to thermal radiation, the temperature of the solar cell is one of the core parameters of the Planck formula and has a strong nonlinear characteristic. The traditional iterative solution method is used to calculate the temperature of the solar cell. The combined equations (2-1) to (2-7) are solved iteratively through Matlab program writing. The specific steps are as follows:
[0064] 1) Start the program and initialize variables;
[0065] 2) Input environmental parameters and structural parameters, including ambient temperature T a , atmospheric spectral transmittance t(λ), solar radiation heating power q, total heat transfer coefficient h c , spectral characteristics of solar cells, etc.;
[0066] 3) Assign an initial value T to the temperature of the solar cell cell =T0, using the initial value and the environmental parameters and structural parameters input in the previous step to calculate the thermal radiation power P of the solar cell itself rad (T cell ), the thermal radiation P absorbed by the solar cell from the atmosphere atm (T a ), and then based on the convection / conduction heat dissipation power P of the solar cell and the ambient air con (T cell , T a ) expression to calculate the solar cell temperature T cell =T1;
[0067] 4) Compare the difference between the calculated value T1 of the solar cell temperature and the previous temperature value T0 to see if they meet the accuracy requirements. The absolute value of the relative error is selected as the accuracy criterion. If the accuracy requirements are met, the data is saved and output. Otherwise, the solar cell temperature value is updated for iterative calculation until the accuracy meets the requirements.
[0068] 5) Save and output the steady-state temperature value of the solar cell;
[0069] 6) End the program.
[0070] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0071] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A bending-resistant insulating epoxy composite heat dissipation film for solar energy, comprising an epoxy composite film body (1), characterized in that: The epoxy composite film body (1) comprises an epoxy resin surface film (101), an epoxy resin bottom film (102), a crystalline silicon radiation layer (103) and a convection grid pad layer (104); the convection grid pad layer (104) is arranged above the epoxy resin bottom film (102); the crystalline silicon radiation layer (103) is arranged above the convection grid pad layer (104); and the epoxy resin surface film (101) is arranged above the crystalline silicon radiation layer (103); The crystalline silicon radiation layer (103) comprises a crystalline polygonal pyramid (1031), the crystalline polygonal pyramid (1031) comprises an incident plate (1032) and a refraction plate (1033), the refraction plate (1033) is arranged above the incident plate (1032), and there are four refraction plates (1033); The convection grille cushion layer (104) comprises a heat-insulating adhesive mesh (1041), and heat-dissipating convection grooves are arranged between the heat-insulating adhesive mesh (1041).
2. The bending-resistant insulating epoxy composite heat dissipation film for solar energy according to claim 1, characterized in that: The outer surface of the epoxy resin surface film (101) is provided with a heat-conducting coating, and the outer surface of the epoxy resin base film (102) is provided with a heat-conducting grease.
3. A production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy, which is realized based on the bending-resistant insulating epoxy composite heat dissipation film for solar energy according to claim 2, wherein: The steps include: Step 1: Pour the selected epoxy resin particles into an ultrasonic cleaning machine for cleaning to remove excess dust on the surface. After cleaning, put the resin particles into a dryer to remove residual moisture on the surface. The drying temperature is 150-160°C and the drying time is 3-4 hours. Step 2: Add the dried resin particles together with the additives into the blow molding machine for heating at a temperature of 320-450°C. After the raw materials are melted, they are stirred by the stirring structure inside the blow molding machine at a speed of 600-800r / min. Step 3: After stirring evenly, the liquid raw material is extruded into a mold by an extruder, the temperature of the extruder head is 210-280° C., and the extruded raw material is stretched and then formed into an epoxy resin surface film (101) and an epoxy resin base film (102) in two steps, wherein the thickness of the epoxy resin surface film (101) is smaller than that of the epoxy resin base film (102); Step 4: Mix the silicon source containing silicon dioxide, water, structure directing agent and alkali in a certain proportion, put them into a pressure-resistant reactor and seal them, then heat them to 100-220°C and keep the temperature constant for 5-10 hours. After the reaction is completed, cool the reactor quickly; Step 5: washing the reaction product with water until the pH value is 8-11, and drying the reaction product to obtain raw powder, pouring the raw powder into a special mold, and then placing the mold and the raw powder into a tube furnace for roasting and activation, and naturally cooling to room temperature after sintering, thereby obtaining a crystalline polygonal pyramid (1031); Step 6: Covering one side surface of the epoxy resin base film (102) with a convection grille cushion layer (104), the convection grille cushion layer (104) being made of a high-transmittance soft rubber material, and then laying a crystal polygonal pyramid (1031) on top of the convection grille cushion layer (104), with the position of the pyramid corresponding to the convection mesh surface groove (1042); Step 7: After the laying is completed, the epoxy resin base film (102) and the crystal polygonal pyramid (1031) are placed in the mold frame, and the adhesive liquid is injected into the surface of the crystal polygonal pyramid (1031). The adhesive filling height is consistent with the cone height, and finally the epoxy resin surface film (101) is covered on the top of the crystal polygonal pyramid (1031); Step 8: Use a hot pressing plate to perform hot pressing on the entire composite membrane structure to allow the glue to melt and infiltrate the membrane structure. After the hot pressing is completed, the composite membrane is taken out and cooled naturally. At this time, the internal crystal polygonal pyramid (1031) can form a group of crystalline silicon radiation layers (103) after being filled with glue and cooled.
4. The production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy according to claim 3, characterized in that: In the step three, in the process of preparing the epoxy resin base film (102), silver powder needs to be added to the raw material, and the ratio of silver powder to raw material is 1:50, wherein the particle size of the silver powder is 0.5-0.7 μm, and its shape is a flake or polygonal structure.
5. The production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy according to claim 3, characterized in that: In the step 5, the diameter of the crystal polygonal pyramid (1031) is 250 μm and the height is 250 μm.
6. The production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy according to claim 3, characterized in that: In the step six, when laying the crystal polygonal pyramid (1031) structure, a filling gap needs to be reserved between the crystal polygonal pyramids (1031), and the width of the filling gap is 0.1 mm.
7. The production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy according to claim 3, characterized in that: In the step seven, after the crystal polygonal pyramid (1031) is laid, the redundant part of the base film needs to be cut off, and then the edge wrapping operation is performed after the cutting, and the raw material structure required for the edge wrapping is consistent with the base film.
8. The production process of a bending-resistant insulating epoxy composite heat dissipation film for solar energy according to claim 3, characterized in that: In the step eight, the thickness of the composite film is 280-290 μm.