A red light-heat-activated delayed fluorescent material based on diphenylethynyl anthracene derivatives and its preparation method and application

By designing red-light thermal activation delayed fluorescent materials of diphenylacetylene anthracene derivatives, the problem of low efficiency of long-band TADF materials is solved, and efficient fluorescent quantum yield and red light emission are achieved. It is suitable for wet OLED devices. Efficient electroluminescent performance.

CN115850098BActive Publication Date: 2024-11-05SUZHOU 30 BILLION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211482813.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-11-05
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

The medium and long-band TADF materials in the prior art are not efficient enough, have few electron acceptor selection, low fluorescence quantum yield, and lack high-efficiency long-band TADF materials suitable for wet preparation.

Method used

Red light-thermal activation delayed fluorescent material designed with diphenylacetylene anthracene derivatives, by using 1,8-dichloro-9,10-bis(phenylacetylene)anthracene and 4-methoxy-N-(4- Methoxyphenyl)-N-(4-(4,4,5,5-tetramethyl-1,3,2-benzene borate-2-yl)aniline and potassium carbonate in a specific ratio The reaction was carried out, and tetratriphenylphosphine palladium was added and purified by column chromatography to form a material with a highly twisted and rigid structure, which was suitable for the preparation of wet OLED devices.

Benefits of technology

It achieves 100% intra-theoretical quantum efficiency, has good conjugation system and charge transfer capabilities, realizes red light emission, and the highest external quantum efficiency reaches 10.1%, showing superior electroluminescent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115850098B_ABST
    Figure CN115850098B_ABST
Patent Text Reader

Abstract

The present invention discloses a red light thermally activated delayed fluorescent material based on diphenylethynyl anthracene derivatives and its preparation method and application, belonging to the technical field of organic optoelectronic materials and devices. The structural formula of the red light thermally activated delayed fluorescent material is #imgabs0#. The material has the following characteristics: ① The molecule has a good conjugated system to ensure good intramolecular charge transfer, which is conducive to the red shift of the molecular emission wavelength to achieve long-wavelength luminescence; ② The electron acceptor ethynyl and electron donor methoxy triarylamine of the molecule show a highly twisted rigid structure, so that the molecule has a very small energy gap difference, thereby achieving a 100% theoretical internal quantum efficiency; ③ The molecule has a high relative molecular mass and the solubility of triarylamine, which ensures that the molecule has good film-forming properties and is suitable for the production of wet-process OLED devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic optoelectronic materials and devices, and specifically relates to a red light thermally activated delayed fluorescent material based on diphenylethynyl anthracene derivatives, and a preparation method and application thereof. Background Art

[0002] Organic light-emitting diodes (OLEDs) have been favored by people in the past few decades because of their good commercialization potential in the fields of mobile phone screens, flat panel displays and solid-state lighting. As the core part of OLEDs, luminescent materials have always been the focus of research for many scientific researchers. Thermally activated delayed fluorescence (TADF) materials have the characteristics of not containing organic precious metals and achieving 100% theoretical internal quantum efficiency by using triplet exciton anti-gap crossing. They have been considered to be the third generation of organic electroluminescent materials after the first generation of traditional fluorescent materials and the second generation of phosphorescent materials. So far, a large number of highly efficient vapor-deposited TADF materials have been successfully developed. In contrast, the wet method is usually simple in process and low in cost, and has obvious advantages in large-area and flexible devices. However, there is little development of TADF materials that can be prepared by wet method, especially long-wavelength TADF materials.

[0003] Generally speaking, TADF materials with high emission efficiency meet the following conditions: ① The highest occupied molecular orbital (HOMO) and the lowest occupied molecular orbital (LUMO) of the molecule can be effectively separated, thus ensuring that the molecule has a small energy gap (∆E ST ); ② The molecule has good charge transfer ability, ensuring that the molecule has a high fluorescence quantum yield. The reason for the slow development of TADF materials with high efficiency and long-wave emission is that according to the energy gap theory, the rate of non-radiative transition of luminescent molecules increases with the red shift of the luminescent wavelength, while the rate of radiative transition decreases. At present, reports on highly efficient long-wavelength emission from vapor-deposited TADF materials mainly focus on introducing strong electron acceptors, such as phthalonitrile (Nature, 2012, 492, 234), tribenazine (Chem. Mater., 2013, 25, 3766), anthraquinone (J. Am. Chem. Soc., 2014, 136, 18070), dicyanopyrazine (Adv. Funct. Mater., 2016, 26, 1813), naphthalimide (Dyes Pigm., 2017,144, 212), etc., to achieve efficient charge transfer and long-wavelength emission. However, there has been no report on the construction of highly efficient long-wavelength emission TADF materials using weak electron acceptors. Summary of the invention

[0004] In view of the problems in the prior art such as the low efficiency of long-wave TADF materials, the limited selection of electron acceptors, and the low fluorescence quantum yield, the present invention provides a red light-heat-activated delayed fluorescence material of a diphenylethynyl anthracene derivative and its preparation method and application. The material has a good conjugated system, and the electron acceptor and electron donor units exhibit a highly twisted rigid structure, and can achieve a theoretical internal quantum efficiency of 100%. At the same time, the material has a high relative molecular mass and the solubility of triarylamine, ensuring that the molecule has good film-forming properties and is suitable for wet-process preparation of OLED devices.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] The first object of the present invention is to provide a red light-heat-activated delayed fluorescent material based on diphenylethynyl anthracene derivatives, the structural formula of which is , named DBP-2MOTPA.

[0007] The second object of the present invention is to provide a method for preparing the red light thermally activated delayed fluorescent material as described in the first object, comprising the following steps:

[0008] 1,8-dichloro-9,10-di(phenylethynyl)anthracene, 4-methoxy-N-(4-methoxyphenyl)-N-(4-(4,4,5,5-tetramethyl-1,3,2-phenylboronic acid pinacol ester-2-yl)phenyl)aniline, and potassium carbonate are weighed in a molar ratio of 1:(2-4):(4-8); added to a mixed solution of toluene, ethanol, and water in a volume ratio of 6:3:1 and stirred to dissolve; tetrakistriphenylphosphine palladium is added in a nitrogen atmosphere, and the molar ratio of tetrakistriphenylphosphine palladium to 1,8-dichloro-9,10-di(phenylethynyl)anthracene is (0.1-0.5):1, and reacted at a reaction temperature of 70-90°C and a reaction time of 18-36h. After the reaction is completed, the red light thermally activated delayed fluorescent material is purified by column chromatography; preferably, the eluent of the column chromatography is a mixed solution of petroleum ether and dichloromethane.

[0009] The reaction formula of the preparation method is:

[0010] .

[0011] The third object of the present invention is to provide an application of the red light thermally activated delayed fluorescent material as described in the first object, wherein the red light thermally activated delayed fluorescent material is used to prepare a wet-process organic electroluminescent diode. The steps of preparing a wet-process organic electroluminescent diode are as follows:

[0012] (1) Clean the anode electrode with detergent, distilled water, acetone, and isopropanol respectively, dry it under infrared light, and finally clean it with ultraviolet ozone for half an hour before use;

[0013] (2) Spin coating the hole transport layer material on the anode at a spin coating speed of 2000 rpm. After the spin coating is completed, heat and anneal at a temperature of 120 °C to form a hole transport layer;

[0014] (3) Spin coating a light-emitting material on the hole transport layer at a spin coating speed of 2000 rpm, and after the spin coating is completed, heating and annealing in a glove box filled with nitrogen to form a light-emitting layer; preferably, the light-emitting material may contain a host material in addition to the red light thermally activated delayed fluorescent material, and the light-emitting material may be formed by mixing the red light thermally activated delayed fluorescent material and the host material in different proportions;

[0015] (4) spin coating an alcohol-soluble electron transport layer material on the light-emitting layer as an electron transport layer;

[0016] (5) A cathode is evaporated on the surface of the electron transport layer to obtain a wet-process red light organic electroluminescent diode.

[0017] Preferably, the hole transport layer material prepared in step (2) is PEDOT:PSS, whose structural formula is , with a molecular weight of 8000 g / mol; in step (3), the main material is CBP, whose structural formula is ; The electron transport layer material in step (4) is PO-T2T, whose structural formula is .

[0018] The fourth object of the present invention is to provide an organic electroluminescent diode prepared by applying the red light thermally activated delayed fluorescent material based on the diphenylethynyl anthracene derivative as described in the third object.

[0019] Beneficial effects:

[0020] 1. The electron acceptor ethynyl and electron donor methoxytriarylamine units of the thermally activated delayed fluorescence material based on diphenylethynyl derivatives of the present invention exhibit a highly twisted rigid structure, which gives the material the property of thermally activated delayed fluorescence, ensures that the triplet excitons of the molecule are effectively upconverted to the singlet state, and makes the molecule have a very small energy gap difference, thereby achieving a theoretical internal quantum efficiency of 100%.

[0021] 2. The molecular configuration of the material described in the present invention has a good conjugated system, which ensures good intramolecular charge transfer, which is beneficial to the red shift of the molecular emission wavelength to achieve long-wavelength luminescence, thereby enabling the material to have good TADF performance and very high solid fluorescence quantum efficiency and the luminescent color presents red light emission.

[0022] 3. The present invention uses a weak acetylene electron-withdrawing group, which is different from the conventional strong electron-withdrawing unit, and has a certain novelty in the design of TADF molecules in the long wavelength band.

[0023] 4. The OLED device based on the thermally activated delayed fluorescent material based on the diphenylethynyl derivative described in the present invention exhibits red light emission, with the highest external quantum efficiency reaching 10.1%, showing excellent electroluminescent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the structure of an organic light emitting diode prepared by the present invention;

[0025] The numbers in the figure represent the following: 1. ITO anode; 2. hole transport layer; 3. light-emitting layer; 4. electron transport layer; 5. metal cathode.

[0026] Figure 2 This is the H NMR spectrum of DBP-2MOTPA prepared in Example 1 of the present invention;

[0027] Figure 3 It is the electroluminescence spectrum of the OLED device prepared in Application Examples 1 to 3. DETAILED DESCRIPTION

[0028] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0029] The materials used in the present invention are as follows:

[0030]

[0031] Among them, ITO, Cs2CO3, Al, CBP, PEDOT:PSS and PO-T2T are commercially available.

[0032] Example 1

[0033] Preparation of red light-heat-activated delayed fluorescent material based on diphenylethynyl anthracene derivatives, the structural formula of which is .

[0034] The synthesis method is:

[0035] 1,8-dichloro-9,10-di(phenylethynyl)anthracene, 4-methoxy-N-(4-methoxyphenyl)-N-(4-(4,4,5,5-tetramethyl-1,3,2-phenylboronic acid pinacol ester-2-yl)phenyl)aniline and potassium carbonate were weighed in a molar ratio of 1:2.5:4. The mixture was added to a mixed solution of toluene, ethanol and water in a volume ratio of 6:3:1 and stirred for dissolution. In a nitrogen atmosphere, tetrakistriphenylphosphine palladium was added, and the molar ratio of tetrakistriphenylphosphine palladium to 1,8-dichloro-9,10-di(phenylethynyl)anthracene was 0.1:1. The reaction was carried out at a reaction temperature of 80°C and a reaction time of 24 hours. After the reaction was completed, the red light thermally activated delayed fluorescent material was purified by column chromatography and named DBP-2MOTPA with a yield of 66%.

[0036] The results of its molecular structure analysis are as follows:

[0037] H NMR spectrum Figure 2 , H NMR (600 MHz, CDCl3): 8.73 (d, J = 9 Hz, 2H), 8.24 (d, J = 9 Hz, 1H), 7.82 (d, J = 8.4 Hz, 2H), 7.65 (t, J = 7.8 Hz, 2H),7.54−7.57 (m, 2H), 7.49 (t, J = 6 Hz, 2H), 7.46-7.47 (m, 1H), 7.41 (d, J= 8.4Hz, 2H), 7.22-7.33 (m, 4H), 6.88-7.01 (m, 14H), 6.86 (d, J = 7.8 Hz, 1H),6.72-6.74 (m, 6H), 3.76 (s, 12H).

[0038] Mass spectrum: 984.39.

[0039] Elemental analysis: C: 85.34, H: 5.32, N: 2.84.

[0040] The reaction formula is as follows:

[0041] .

[0042] It should be noted that, in other embodiments, when the experimental process meets the following conditions, the purpose of the present invention can be achieved:

[0043] The molar ratio of 1,8-dichloro-9,10-di(phenylethynyl)anthracene, 4-methoxy-N-(4-methoxyphenyl)-N-(4-(4,4,5,5-tetramethyl-1,3,2-phenylboronic acid pinacol ester-2-yl)phenyl)aniline and potassium carbonate is preferably 1:(2-4):(4-8). In addition to 1:2.5:4 as defined in Example 1, in other embodiments, it can also be designed to be 1:2:4, 1:3:4 or 1:4:8.

[0044] The molar ratio of tetrakistriphenylphosphine palladium to 1,8-dichloro-9,10-di(phenylethynyl)anthracene is preferably (0.1-0.5):1. In addition to 0.1:1 as defined in Example 1, in other embodiments, it can also be designed to be 0.3:1 or 0.5:1.

[0045] The reaction temperature is preferably 70-90°C. In addition to 80°C in Example 1, other embodiments may also be designed to be 70°C or 90°C. As for the reaction time, a higher temperature can increase the reaction rate, so the reaction time can be appropriately shortened; when the temperature is lowered, the reaction time can be appropriately extended.

[0046] For the above process parameters, those skilled in the art can make appropriate selections according to actual needs, all of which can achieve the purpose of the present invention, and examples are not given here one by one.

[0047] Application Example 1

[0048] Preparation of wet red OLED devices:

[0049] The schematic diagram of the device structure is shown in Figure 1 As shown, from bottom to top, it includes an ITO anode 1, a hole transport layer 2, a light-emitting layer 3, an electron transport layer 4, and a metal cathode 5. The hole transport layer material is PEDOT:PSS, the light-emitting layer material is DBP-2MOTPA, and the electron transport layer material is PO-T2T.

[0050] The preparation method of the wet red OLED device is as follows:

[0051] (1) Cleaning of indium tin oxide (ITO) glass substrate: ultrasonically clean ITO using detergent, deionized water, ethanol, acetone, and isopropanol, three times for each solvent, and then dry it under infrared light for 1 hour. Finally, clean it with ultraviolet ozone for half an hour before use.

[0052] (2) Spin coating of hole transport layer: A layer of hole transport layer material PEDOT:PSS (poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid)) was spin coated on the surface of ITO at a speed of 2000 rpm with a film thickness of 40 nm. Then, the substrate was dried on a hot plate at 120°C for 20 min.

[0053] (3) Preparation of the light-emitting layer: After cooling to room temperature, 1,2-dichloroethane containing 10 mg / mL DBP-2MOTPA light-emitting material was spin-coated on PEDOT:PSS at a speed of 2000 rpm for 30 seconds to a film thickness of 30 nm. After drying at 200°C in a nitrogen atmosphere for 10 minutes, the film was cooled to room temperature.

[0054] (4) Spin coating of electron transport layer: A layer of PO-T2T material with a concentration of 5 mg / mL and a film thickness of 40 nm was spin coated on the surface of the light-emitting layer at a speed of 2000 rpm. Then, the substrate was dried on a hot plate at 120 °C for 20 min.

[0055] (5) Evaporation deposition of cathode: Cs2CO3 and Al were evaporated as cathode at rates of 0.2 Å / s and 10 Å / s, respectively.

[0056] Device performance test: In a glove box, a Kethiey 2400 semiconductor performance test system connected to an ST-86LA screen brightness meter was used to measure the brightness-current-voltage curve of the device. At the same time, a PR655 spectrometer was used to test the electroluminescence spectrum and color coordinates.

[0057] The device performance is as follows: the turn-on voltage is 4.8 V and the maximum brightness is 1522 cd / m 2 , the color coordinates are (0.66, 0.33) and the maximum external quantum efficiency is 2.6%.

[0058] Application Example 2

[0059] A wet-process red light OLED device was prepared according to the method in Application Example 1. The difference from Application Example 1 was that in Application Example 2, CBP main material was added in the preparation of the light-emitting layer, and the mass ratio of DBP-2MOTPA:CBP was 0.06:1.

[0060] The device performance is as follows: the lighting voltage is 4.5 V and the maximum brightness is 4015 cd / m 2 , the color coordinates are (0.61, 0.37) and the maximum external quantum efficiency is 10.1%.

[0061] Application Example 3

[0062] A wet-process red light OLED device was prepared according to the method in Application Example 1. The difference from Application Example 1 is that in Application Example 3, a CBP main material is added in the preparation of the light-emitting layer, and the mass ratio of DBP-2MOTPA:CBP is 0.1:1.

[0063] The device performance is as follows: the lighting voltage is 4.6 V and the maximum brightness is 3188 cd / m 2 , the color coordinates are (0.61, 0.38) and the maximum external quantum efficiency is 7.9%.

[0064] Figure 3 is the electroluminescence spectrum of the OLED device prepared in Application Examples 1 to 3, from Figure 3 It can be seen that in Application Examples 1 to 3, the maximum emission wavelengths of the electroluminescent spectra are 680 nm, 640 nm and 644 nm, respectively, showing red light emission.

[0065] The above is a detailed introduction to the synthesis method and application of a red light thermally activated delayed fluorescent molecule provided by the present invention. Specific examples are cited herein to illustrate the present invention and its implementation, but these examples are not intended to limit the present invention. Any simple modification of the present invention without departing from the principle of the present invention also falls within the scope of protection of the claims of the present invention.

Claims

1. A red light-heat-activated delayed fluorescent material based on diphenylethynyl anthracene derivatives, characterized in that: Its structural formula is .

2. The method for preparing a red light-heat-activated delayed fluorescent material based on a diphenylethynyl anthracene derivative according to claim 1, characterized in that: The specific preparation method is as follows: 1,8-Dichloro-9,10-di(phenylethynyl)anthracene, 4-methoxy-N-(4-methoxyphenyl)-N-(4-(4,4,5,5-tetramethyl-1,3,2-phenylboronic acid pinacol ester-2-yl)phenyl)aniline and potassium carbonate are added to a mixed solution consisting of toluene, ethanol and water, and stirred to dissolve; tetrakistriphenylphosphine palladium is added in a protective gas atmosphere, and the reaction is carried out at a temperature of 70-90°C for 18-36h. After the reaction is completed, the target product is purified by column chromatography.

3. The method for preparing a red light-heat-activated delayed fluorescent material based on a diphenylethynyl anthracene derivative according to claim 2, characterized in that: The molar ratio of the 1,8-dichloro-9,10-di(phenylethynyl)anthracene, 4-methoxy-N-(4-methoxyphenyl)-N-(4-(4,4,5,5-tetramethyl-1,3,2-phenylboronic acid pinacol ester-2-yl)phenyl)aniline and potassium carbonate is 1:(2-4):(4-8); the volume ratio of toluene, ethanol and water is 6:3:1; the molar ratio of tetrakistriphenylphosphine palladium to 1,8-dichloro-9,10-di(phenylethynyl)anthracene is (0.1-0.5):

1.

4. The method for preparing a red light-heat-activated delayed fluorescent material based on a diphenylethynyl anthracene derivative according to claim 2, characterized in that: The eluent of the column chromatography method is a mixed solution of petroleum ether and dichloromethane.

5. The use of a red light thermally activated delayed fluorescent material based on a diphenylethynyl anthracene derivative as claimed in claim 1, characterized in that: The red light thermally activated delayed fluorescent material is used for preparing wet-process organic electroluminescent diodes.

6. The use of a red light thermally activated delayed fluorescent material based on a diphenylethynyl anthracene derivative according to claim 5, characterized in that: The steps of preparing the wet organic light emitting diode are as follows: (1) Clean the anode electrode with detergent, distilled water, acetone, and isopropyl alcohol respectively, dry it under infrared light, and finally clean it with ultraviolet ozone for later use; (2) Spin coating a hole transport layer material on the anode, and then performing heating annealing to form a hole transport layer; (3) Spin coating a light-emitting material containing a red light-heat-activated delayed fluorescent material on the hole transport layer, and after the spin coating is completed, placing it in a protective gas atmosphere for heating and annealing to form a light-emitting layer; (4) Spin coating a layer of electron transport layer material on the light-emitting layer, and then heating and annealing the layer to form an electron transport layer; (5) A cathode is evaporated on the surface of the electron transport layer to obtain a wet-process red light organic electroluminescent diode.

7. The use of a red light thermally activated delayed fluorescent material based on a diphenylethynyl anthracene derivative according to claim 6, characterized in that: The heating annealing temperature in step (2) and step (4) is 120°C; the protective gas in step (3) is nitrogen, and the heating annealing temperature is 200°C.

8. The use of a red light thermally activated delayed fluorescent material based on a diphenylethynyl anthracene derivative according to claim 6, characterized in that: The hole transport layer material in step (2) is PEDOT:PSS, and its structural formula is , with a molecular weight of 8000 g / mol; the electron transport layer material in step (4) is PO-T2T, whose structural formula is .

9. The use of a red light thermally activated delayed fluorescent material based on a diphenylethynyl anthracene derivative according to claim 6, characterized in that: The luminescent material containing the red light thermally activated delayed fluorescent material in step (3) also includes a host material; the host material is CBP, and its structural formula is ; The mass ratio of the red light thermally activated delayed fluorescent material to the main material is (0.06-0.1):

1.

10. An organic electroluminescent diode prepared by using the red light thermally activated delayed fluorescent material based on the diphenylethynyl anthracene derivative according to any one of claims 5 to 9.