Preparation of a new type of pyridine carboxylic acid ligand and its rare earth complex luminescent material
Through the coordination of the novel pyridine carboxylic acid ligand UPA with rare earth ions Eu3+ and Tb3+, an efficient rare earth complex luminescent material was prepared, which solved the problem of low luminescence efficiency of rare earth luminescent materials in the prior art, and achieved bright colors and long The fluorescence performance of life span has expanded its application prospects.
Patent Information
- Application Number
- CN202211607945.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-14
AI Technical Summary
The luminescence efficiency of existing rare earth luminescent materials is not ideal, mainly due to the low chelation ability of the ligand and the presence of coordination water molecules, it is difficult to construct rare earth complexes with luminescent properties.
Develop a new pyridine carboxylic acid ligand-2-(6-ureidopyridine carboxylic acid)-ethyl ester (UPA), to prepare high-stability rare earth complexes through specific synthetic methods, using UPA and rare earth ions Eu3+ and Tb3+ coordinate to form a sensitized luminescent material.
The prepared rare earth complex has bright colors, long fluorescence lifetime and good fluorescence performance. It is suitable for energy conservation and environmental protection, electronic information, agriculture and medicine and other fields, significantly improving the luminescence efficiency of rare earth ions.
Smart Images

Figure CN115850164B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of photoluminescent materials, and in particular to the preparation of a novel pyridinecarboxylic acid ligand and a rare earth complex luminescent material. Background Art
[0002] Photoluminescent materials have attracted extensive attention due to their potential application value in energy conservation and environmental protection, electronic information, agriculture, medicine, etc. Rare earth-based luminescent materials are considered to be an ideal luminescent material due to their high purity, bright color and long life. The excellent performance of rare earth luminescent materials all originates from the transition of 4f electrons between different energy levels: ff transition, that is, energy level transition within f configuration; fd transition, that is, energy level transition between 4f-5d configuration; charge transfer transition. The luminescence of rare earth ions can be roughly divided into three processes: ① receiving external energy to be excited; ② electrons transition from the ground state to the excited state; ③ when electrons return from the excited state to the energy level with lower energy, they release radiation energy and emit fluorescence. Although the luminescence of rare earth ions has an emission peak with a fixed wavelength, a narrow emission spectrum and high color purity, the ff transition of rare earth ions is forbidden, so the absorption coefficient of rare earth ions in the ultraviolet region is small, resulting in less than ideal luminescence efficiency. The existing known technology is to use the "Antenna effect" (ie, "antenna effect") to transfer energy absorbed by other groups (ligands) to rare earth ions, thereby sensitizing the rare earth ions to emit light, and the luminescence efficiency of the rare earth ions is greatly enhanced.
[0003] Among the existing disclosed organic ligands, there are many with strong chelating ability, for example, they can be used for the binding and separation of metal ions, but these ligands are not suitable for constructing luminescent rare earth complexes, because the complexes formed after these ligands chelate with rare earth ions do not have luminescent properties or are difficult to achieve luminescence. The reason is that there are many factors that affect the energy transfer of the Antenna effect, such as the absorption capacity of the ligand, the match between the ligand and the resonant emission energy level of the rare earth ion, temperature, the number of coordinated water molecules, etc. Among them, the presence of coordinated water molecules can cause the vibration of the OH bond to lose energy, and the fluorescence efficiency of the complex is reduced. Therefore, it is still a challenge to develop organic ligands with strong chelating ability and effectively form luminescent complexes with rare earth ions. Summary of the invention
[0004] The present invention provides a method for preparing a novel pyridinecarboxylic acid ligand for sensitizing rare earth ions to emit light, and prepares a rare earth complex luminescent material with high stability based on the compound as a ligand.
[0005] The novel pyridine carboxylic acid ligand of the present invention is: 2-(6-ureidopyridine carboxylic acid)-ethyl methacrylate, referred to as UPA; its structural formula is:
[0006]
[0007] The preparation method of the novel pyridine carboxylic acid ligand comprises the following steps:
[0008] 1) In a round-bottom flask, add methyl 6-aminopyridine-2-carboxylate, isocyanoethyl methacrylate, and pyridine in sequence, stir magnetically to mix evenly, reflux at 100-120° C. for 1-3 hours, and then cool to room temperature, wherein the molar ratio of methyl 6-aminopyridine-2-carboxylate to isocyanoethyl methacrylate is 1:1.3-1:1.5;
[0009] 2) The reaction solution was allowed to stand, filtered, washed with a large amount of petroleum ether, and the solid was collected and vacuum dried to obtain the product methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester;
[0010] 3) tetrahydrofuran, water and sodium hydroxide are added to a round-bottom flask in sequence, and after being mixed evenly by magnetic stirring, methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester obtained in step 2) is added, and the mixture is reacted at room temperature for 10 to 30 minutes, and a dilute hydrochloric acid solution is added to adjust the reaction system to acidity, and the organic solvent is removed by extraction, and the mixture is filtered, washed with deionized water, and vacuum dried to obtain a white solid product UPA, which is refrigerated for later use; wherein the volume ratio of tetrahydrofuran to water is 2:1 to 1:2, the molar concentration of the sodium hydroxide solution is 1.0 to 1.5 mol / L, and the molar concentration of the methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester solution is 1.5 to 1.7 mmol / L.
[0011] The synthetic route of UPA is as follows Figure 1 shown.
[0012] The ligand methacrylate-2-(6-ureidopyridinecarboxylic acid)-ethyl ester (UPA) prepared by the present invention is prepared by using liquid 1 HNMR, 13 C NMR experiment characterized its chemical structure, and its NMR spectrum and chemical shift assignment are as follows Figure 2 and Figure 3 In addition, since UPA is a new compound, ESI-HRMS test was also performed to further determine its structure. Figure 4 As shown, in negative ion mode, M[C 13 H 14 N 3 O 5 ] - The theoretical value is 292.0933, and the signal peak 292.0925 was captured, which proved that UPA was successfully prepared.
[0013] Using 2-(6-ureidopyridinecarboxylic acid)-ethyl methacrylate (UPA) as a ligand, the fluorescence titration method was used to determine the relative molecular mass of UPA and rare earth ion Eu in aqueous solution. 3+ and Tb 3+ The coordination number, UPA sensitized rare earth ions to emit light, and a rare earth complex was prepared. The luminescent material has bright color, a long fluorescence lifetime, and good fluorescence performance, which is conducive to further commercial application.
[0014] The method for preparing a rare earth complex luminescent material using the novel pyridine carboxylic acid ligand comprises the following steps:
[0015] At room temperature, UPA, water and potassium hydroxide are sequentially added into a round-bottom flask, and 0.033-0.957 eq of rare earth ion europium nitrate or terbium nitrate solution of the same concentration is added dropwise, and after magnetic stirring and mixing evenly, rare earth complex luminescent materials with different luminescent intensities are prepared; wherein the molar ratio of UPA to potassium hydroxide is 1:1, and the molar concentration is 0.999×10-5-1.001×10-5 mol / L.
[0016] The beneficial effects of the present invention are as follows: a novel pyridinecarboxylic acid ligand and its rare earth complex luminescent material of the present invention are prepared by using cheap and readily available chemicals on the market as raw materials, and a novel pyridinecarboxylic acid ligand: methyl acrylate-2-(6-ureidopyridinecarboxylic acid)-ethyl ester (UPA) is prepared; methyl acrylate-2-(6-ureidopyridinecarboxylic acid)-ethyl ester (UPA) is used as a ligand, and the fluorescence titration method is used to respectively study and determine the UPA and rare earth ion Eu in aqueous solution. 3+ and Tb 3+ Coordination number, UPA sensitizes rare earth ions to emit light, and the prepared rare earth complex luminescent material has bright color, long fluorescence lifetime, good fluorescence performance, high purity, bright color, long lifetime, and can play an important role in energy conservation and environmental protection, electronic information, agriculture, medicine, etc., and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The schematic diagram is a synthetic route of the novel pyridinecarboxylic acid ligand UPA of the present invention.
[0018] Figure 2 The H NMR spectrum and chemical shift assignment of the UPA ligand prepared in the present invention in deuterated DMSO. “*” represents the proton signal of DMSO (δ iso =2.49ppm) and H 2 The proton signal of O (δ iso =3.33ppm). Figure 3 The carbon NMR spectrum and chemical shift assignment of the UPA ligand prepared in the present invention in deuterated DMSO. "*" represents the solvent signal peak.
[0019] Figure 4 This is the ESI-HRMS spectrum of the UPA ligand prepared in the present invention. 13 H 14 N 3 O 5 ] - The theoretical value is 292.0933, and the signal peak 292.0925 is captured.
[0020] Figure 5 The figure is a graph showing the intensity variation of the fluorescence emission spectrum of Tb-UPA prepared in the present invention at 544 nm.
[0021] Figure 6 The figure is a graph showing the intensity variation of the fluorescence emission spectrum of Eu-UPA prepared in the present invention at 614 nm.
[0022] Figure 7 The Eu-UPA complex luminescent material prepared in the present invention and Eu 3+ Fluorescence spectra of ionic solutions.
[0023] Figure 8 The Tb-UPA complex luminescent material prepared in the present invention and Tb 3+ Fluorescence spectra of ionic solutions. DETAILED DESCRIPTION
[0024] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0025] Embodiment 1:
[0026] Step 1) Preparation of ligand 2-(6-ureidopyridinecarboxylic acid)-ethyl methacrylate (UPA)
[0027] Step 1.1) In a round-bottom flask, add 0.428 g of methyl 6-aminopyridine-2-carboxylate, 0.65 g of isocyanoethyl methacrylate, and 5 ml of pyridine in sequence, stir magnetically to mix well, reflux at 110° C. for 1 h, and then cool to room temperature.
[0028] Step 1.2) The reaction solution was allowed to stand, filtered, washed with 150 ml of petroleum ether, and the solid was collected and dried in vacuo to obtain the product methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester.
[0029] Step 1.3) In a round-bottom flask, add 7.5 ml of tetrahydrofuran, 7.5 ml of water, and 0.05 g of sodium hydroxide in sequence, stir magnetically and mix well, then add 0.25 g of methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester, react at room temperature for 10 min, add dilute hydrochloric acid solution to adjust the reaction system to acidity, remove the organic solvent by desolventizing, filter, wash with deionized water, and vacuum dry to obtain a white solid product UPA, which is refrigerated for later use.
[0030] Step 2) Preparation of rare earth complex luminescent material
[0031] Step 2.1) At room temperature (25°C), the concentration is 1.0*10 -5 M UPA+KOH aqueous solution and Eu(NO 3 ) 3 Solution, take 15 clean reagent bottles with a capacity of 5 ml, measure 15 portions of 2 ml UPA+KOH aqueous solution in parallel and pour them into the reagent bottles, number them in sequence from 1 to 15, and then add 0.033, 0.099, 0.165, 0.231, 0.297, 0.363, 0.429, 0.495, 0.561, 0.627, 0.693, 0.759, 0.825, 0.891, and 0.957 eq of rare earth ion europium nitrate solution respectively, stir magnetically and mix evenly, and then prepare rare earth complex (Eu-UPA) luminescent materials with different luminescence intensities.
[0032] Step 2.2) At room temperature (25°C), the concentration is 1.0*10 -5 M UPA+KOH aqueous solution and Tb(NO 3 ) 3 Solution, take 15 clean reagent bottles with a capacity of 5 ml, measure 15 portions of 2 ml UPA+KOH aqueous solution in parallel and pour them into the reagent bottles, number them in sequence from 1 to 15, and then drop 0.033, 0.099, 0.165, 0.231, 0.297, 0.363, 0.429, 0.495, 0.561, 0.627, 0.693, 0.759, 0.825, 0.891, and 0.957 eq of rare earth ion terbium nitrate solution respectively, stir magnetically and mix evenly to obtain rare earth complex (Tb-UPA) luminescent materials with different luminescence intensities.
[0033] Embodiment 2:
[0034] Step 1) Preparation of ligand 2-(6-ureidopyridinecarboxylic acid)-ethyl methacrylate (UPA)
[0035] Step 1.1) In a round-bottom flask, 0.855 g of methyl 6-aminopyridine-2-carboxylate, 1.3 g of isocyanoethyl methacrylate, and 10 ml of pyridine were added in sequence, and after being mixed evenly by magnetic stirring, the mixture was refluxed at 115° C. for 2 h and then cooled to room temperature.
[0036] Step 1.2) The reaction solution was allowed to stand, filtered, washed with 200 ml of petroleum ether, and the solid was collected and dried in vacuo to obtain the product methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester.
[0037] Step 1.3) In a round-bottom flask, 15 ml of tetrahydrofuran, 7.5 ml of water, and 0.1 g of sodium hydroxide were added in sequence. After magnetic stirring and mixing, 0.5 g of methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester was added, and the mixture was reacted at room temperature for 20 min. A dilute hydrochloric acid solution was added to adjust the reaction system to acidity, and the organic solvent was removed by desolventizing. The mixture was filtered, washed with deionized water, and vacuum dried to obtain a white solid product UPA, which was refrigerated for later use.
[0038] Step 2) Preparation of rare earth complex luminescent material
[0039] Step 2.1) At room temperature (25°C), the concentration is 1.0*10 -5 M UPA+KOH aqueous solution and Eu(NO 3 ) 3 Solution, take 15 clean reagent bottles with a capacity of 5 ml, measure 15 portions of 2 ml UPA+KOH aqueous solution in parallel and pour them into the reagent bottles, number them in sequence from 1 to 15, and then add 0.033, 0.099, 0.165, 0.231, 0.297, 0.363, 0.429, 0.495, 0.561, 0.627, 0.693, 0.759, 0.825, 0.891, and 0.957 eq of rare earth ion europium nitrate solution respectively, stir magnetically and mix evenly to obtain rare earth complex (Eu-UPA) luminescent materials with different luminescence intensities.
[0040] Step 2.2) At room temperature (25°C), the concentration is 1.0*10 -5 M UPA+KOH aqueous solution and Tb(NO 3 ) 3Solution, take 15 clean reagent bottles with a capacity of 5 ml, measure 15 portions of 2 ml UPA+KOH aqueous solution in parallel and pour them into the reagent bottles, number them in sequence from 1 to 15, and then drop 0.033, 0.099, 0.165, 0.231, 0.297, 0.363, 0.429, 0.495, 0.561, 0.627, 0.693, 0.759, 0.825, 0.891, and 0.957 eq of rare earth ion terbium nitrate solution respectively, stir magnetically and mix evenly to obtain rare earth complex (Tb-UPA) luminescent materials with different luminescence intensities.
[0041] Embodiment 3:
[0042] Step 1) Preparation of ligand 2-(6-ureidopyridinecarboxylic acid)-ethyl methacrylate (UPA)
[0043] Step 1.1) In a round-bottom flask, 1.71 g of methyl 6-aminopyridine-2-carboxylate, 2.6 g of isocyanoethyl methacrylate, and 20 ml of pyridine were added in sequence, and after being mixed evenly by magnetic stirring, the mixture was refluxed at 120° C. for 2.5 h and then cooled to room temperature.
[0044] Step 1.2) The reaction solution was allowed to stand, filtered, washed with 250 ml of petroleum ether, and the solid was collected and dried in vacuo to obtain the product methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester.
[0045] Step 1.3) In a round-bottom flask, 30 ml of tetrahydrofuran, 30 ml of water, and 0.2 g of sodium hydroxide were added in sequence. After magnetic stirring and mixing, 1 g of methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester was added, and the mixture was reacted at room temperature for 30 min. A dilute hydrochloric acid solution was added to adjust the reaction system to acidity, and the organic solvent was removed by desolventizing. The mixture was filtered, washed with deionized water, and vacuum dried to obtain a white solid product UPA, which was refrigerated for later use.
[0046] Step 2) Preparation of rare earth complex luminescent material
[0047] Step 2.1) At room temperature (25°C), the concentration is 1.0*10 -5 M UPA+KOH aqueous solution and Eu(NO 3 ) 3Solution, take 15 clean reagent bottles with a capacity of 5 ml, measure 15 portions of 2 ml UPA+KOH aqueous solution in parallel and pour them into the reagent bottles, number them in sequence from 1 to 15, and then add 0.033, 0.099, 0.165, 0.231, 0.297, 0.363, 0.429, 0.495, 0.561, 0.627, 0.693, 0.759, 0.825, 0.891, and 0.957 eq of rare earth ion europium nitrate solution respectively, stir magnetically and mix evenly to obtain rare earth complex (Eu-UPA) luminescent materials with different luminescence intensities.
[0048] Step 2.2) At room temperature (25°C), the concentration is 1.0*10 -5 M UPA+KOH aqueous solution and Tb(NO 3 ) 3 Solution, take 15 clean reagent bottles with a capacity of 5 ml, measure 15 portions of 2 ml UPA+KOH aqueous solution in parallel and pour them into the reagent bottles, number them in sequence from 1 to 15, and then drop 0.033, 0.099, 0.165, 0.231, 0.297, 0.363, 0.429, 0.495, 0.561, 0.627, 0.693, 0.759, 0.825, 0.891, and 0.957 eq of rare earth ion terbium nitrate solution respectively, stir magnetically and mix evenly to obtain rare earth complex (Tb-UPA) luminescent materials with different luminescence intensities.
[0049] The ligand methacrylate-2-(6-ureidopyridinecarboxylic acid)-ethyl ester (UPA) prepared by the present invention is prepared by using liquid 1 HNMR, 13 C NMR experiment characterized its chemical structure, and its NMR spectrum and chemical shift assignment are as follows Figure 2 and Figure 3 In addition, since UPA is a new compound, ESI-HRMS test was also performed to further determine its structure. Figure 4 As shown, in negative ion mode, M[C 13 H 14 N 3 O 5 ] - The theoretical value is 292.0933, and the signal peak 292.0925 was captured, which proved that UPA was successfully prepared.
[0050] like Figure 7 As shown, the emission spectrum excitation wavelength is 280nm. From the emission spectrum, there are obvious emission peaks at 578nm, 592nm, 614nm, 652nm and 703nm. This is Eu 3+ The five characteristic emission peaks correspond to Eu3+ of 5 D 0 → 7 F J (J = 0, 1, 2, 3, 4) transitions, among which the peak at 613nm is the most obvious, corresponding to 5 D 0 → 7 F 2 The intensity of the transition emission peak is the largest. 3+ The ratio of the amount of UPA to the fluorescence emission peak intensity (at 614 nm) is plotted, and a clear inflection point appears near 0.363. 3+ Formation of a 3:1 complex (such as Figure 6 As shown), with rare earth ion Eu 3+ For example, the structural formula of the rare earth complex luminescent material prepared by the present invention is as follows:
[0051]
[0052] In addition, the same method was used to obtain the relationship between UPA and rare earth ion Tb in aqueous solution. 3+ Formation of a 2:1 complex (eg Figure 5 As shown). With rare earth ion Tb 3+ For example, the structural formula of the rare earth complex luminescent material prepared by the present invention is as follows:
[0053]
[0054] In addition, it is worth noting that Figure 7 and 8 As shown, under the same conditions, UPA and rare earth ion Eu are present at the same time. 3+ or Tb 3+ The fluorescence emission intensity of the aqueous solution is significantly stronger than that of the pure rare earth ion aqueous solution, which indicates that the coordination effect of UPA and rare earth ions prevents the interference of external water molecules, sensitizes the luminescence of rare earth ions, and enhances the fluorescence intensity of the solution.
Claims
1. A pyridine carboxylic acid ligand, characterized in that: The pyridine carboxylic acid ligand is: methyl acrylate-2-(6-ureidopyridine carboxylic acid)-ethyl ester, referred to as UPA; its structural formula is: 。 2. A method for preparing a pyridinecarboxylic acid ligand according to claim 1, characterized in that: The preparation method thereof comprises the following steps: 1) In a round-bottom flask, add methyl 6-aminopyridine-2-carboxylate, isocyanoethyl methacrylate, and pyridine in sequence, stir magnetically to mix evenly, reflux at 100-120°C for 1-3 hours, and then cool to room temperature, wherein the molar ratio of methyl 6-aminopyridine-2-carboxylate to isocyanoethyl methacrylate is 1:1.3-1:1.5; 2) The reaction solution was allowed to stand, filtered, washed with a large amount of petroleum ether, the solid was collected, and vacuum dried to obtain the product methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester; 3) In a round-bottom flask, tetrahydrofuran, water, and sodium hydroxide are added in sequence. After being evenly mixed by magnetic stirring, methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester obtained in step 2) is added, and the mixture is reacted at room temperature for 10 to 30 min. A dilute hydrochloric acid solution is added to adjust the reaction system to acidity, and the organic solvent is removed by extraction. The mixture is filtered, washed with deionized water, and vacuum dried to obtain a white solid product UPA, which is refrigerated for later use. The volume ratio of tetrahydrofuran to water is 2:1 to 1:2, the molar concentration of the sodium hydroxide solution is 1.0 to 1.5 mol / L, and the molar concentration of the methyl methacrylate-2-(6-ureidopyridinecarboxylic acid methyl ester)-ethyl ester solution is 1.5 to 1.7 mmol / L.
3. A method for preparing a rare earth complex luminescent material using the pyridinecarboxylic acid ligand according to claim 1 or the pyridinecarboxylic acid ligand prepared by the preparation method according to claim 2, characterized in that: The following steps are involved: At room temperature, UPA, water and potassium hydroxide are added to a round-bottom flask in sequence, and 0.033 to 0.957 equivalents of rare earth ion europium nitrate or terbium nitrate solution of the same concentration are added dropwise, and after magnetic stirring and mixing evenly, rare earth complex luminescent materials with different luminescent intensities are prepared; wherein the molar ratio of UPA to potassium hydroxide is 1:1, and the molar concentration is 0.999×10-5 to 1.001×10-5 mol / L.
Citation Information
Patent Citations
Nd(III) compound light-emitting material containing modified imidazole carboxylic acid and pyridine carboxylic acid mixed ligand and preparation method of Nd(III) compound light-emitting material
CN109824706A