A method for preparing a high barrier biodegradable film

By using biodegradable materials such as PBAT, polypropylene carbonate, and dimethyl carbonate-butylene glycol-organic acid copolymer, combined with inorganic nanomaterials and antioxidants, the preparation process of high-barrier biodegradable films is simplified , solving the problems of complex processes and high costs in the existing technology, and achieving efficient and environmentally friendly film preparation.

CN115850760BActive Publication Date: 2024-10-25JINCHUAN GROUP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211674493.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-10-25
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

The existing high-barrier biodegradable films have complex preparation processes and high production costs, making them difficult to be widely used in packaging, medical, food and other fields.

Method used

Using biodegradable materials such as PBAT, polypropylene carbonate, dimethyl carbonate-butylene glycol-organic acid copolymer, plasticizer, inorganic nanomaterials and antioxidants, it is extruded through a high-speed mixer and twin-screw extruder The machine prepares high-barrier biodegradable films, simplifying the process and reducing production costs.

Benefits of technology

The preparation of high-barrier biodegradable films is achieved, which simplifies the process and reduces production costs. The material is biodegradable and will not cause pollution to the environment, so it has good development prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 38128DEST_PATH_IMAGE001
    Figure 38128DEST_PATH_IMAGE001
Patent Text Reader

Abstract

The present invention discloses a method for preparing a high-barrier biodegradable film, wherein PBAT, polypropylene carbonate, dimethyl carbonate-butylene glycol-organic acid copolymer, etc. are all biodegradable materials and will not cause white pollution to the environment. The barrier properties of the film are improved by using two types of materials, polypropylene carbonate and dimethyl carbonate-butylene glycol-organic acid copolymer; and the shortcomings of the melt adhesion mold are improved by adding inorganic nanomaterials. The biodegradable film of the present invention has simple processing conditions, good barrier properties, and good development prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a method for preparing a high-barrier biodegradable film. Background Art

[0002] High barrier materials have the characteristics of oxygen barrier, gas barrier, oil barrier, etc. They can prevent the invasion of external substances and keep the internal environment of the package stable. They are widely used in packaging, medical, food, agriculture and other fields. At present, high barrier materials include metal, glass, polymer materials, etc., among which representative polymer film materials include polyvinylidene fluoride, polyvinylidene chloride, etc. Although polyvinylidene chloride and polyvinylidene fluoride have good barrier properties, they are not degradable, and long-term use is bound to cause environmental pollution problems.

[0003] Polybutylene terephthalate-adipate-butylene terephthalate (PBAT) is currently an internationally recognized biodegradable resin. Using PBAT as a key material, the development of biodegradable high-barrier films has been one of the research hotspots in recent years. CN106881929A discloses a high-barrier composite film composed of PBAT and starch. The film adopts a sandwich structure, using starch nanocomposite materials as the sandwich layer and PBAT materials as the outer layer to form a multi-layer composite film to improve the barrier properties. However, this method has a complex process, a long production process, involves a large number of equipment, and a large investment. CN113211920 discloses a multi-layer co-extruded fully degradable high-barrier packaging film and a preparation method thereof. The packaging film consists of five layers: the first layer is an outer protective layer A, which is a blend of PLA, PBAT, carbodiimide anti-hydrolysis agent and anti-ultraviolet agent; the second layer is an adhesive layer B, which is a blend of PLA and a multi-active functional group compatibilizer; the third layer is a high-barrier layer C, which is PGA; the fourth layer is an adhesive layer D, which is a blend of PLA and a multi-active functional group compatibilizer; the fifth layer is a heat-sealing layer E, which is a blend of PLA and PCL. Similarly, this method is relatively complicated to process, the equipment is expensive, and the production cost is high. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a high barrier biodegradable film, so as to solve the problems of complex preparation process and high production cost of the high barrier biodegradable film in the above-mentioned background technology.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A method for preparing a high-barrier biodegradable film comprises the following steps:

[0007] S1: Add 30-55 parts of PBAT, 1-10 parts of polypropylene carbonate, 2-5 parts of plasticizer, 0.1-1 part of heat stabilizer and 0.1-1 part of antioxidant into a high-speed mixer, set the speed of the high-speed mixer to 800-1500 rpm, mix for 5-20 minutes, and obtain premix A;

[0008] S2: 30 to 55 parts of PBAT, 1 to 10 parts of dimethyl carbonate-butylene glycol-organic acid copolymer, 2 to 5 parts of plasticizer, 0.5 to 3 parts of 5-hydroxymethyl-2-furancarboxylic acid and 0.1 to 1 part of antioxidant are added into a high-speed mixer, and the speed of the high-speed mixer is set to 800 to 1500 rpm to obtain premix B;

[0009] S3: adding premix A, premix B and 2-8 parts of inorganic nanomaterials, 0.1-1 part of light stabilizer and 0.1-1 part of antioxidant into a high-speed mixer, setting the speed of the high-speed mixer to 800-1500 rpm to obtain a mixture;

[0010] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain high-barrier biodegradable granules;

[0011] S5: Dry the high barrier biodegradable particles at 50°C-80°C for 2-8 hours, and then process them in a film blowing machine at 160°C-240°C to obtain a high barrier biodegradable film.

[0012] The number average molecular weight of the PBAT is 50,000 to 150,000.

[0013] The number average molecular weight of the polypropylene carbonate is 80,000 to 150,000.

[0014] The plasticizer is at least one of polyethylene glycol, triethyl citrate, acetyl tri-n-butyl citrate, epoxy soybean oil, and triacetin.

[0015] The heat stabilizer is at least one of barium stearate, calcium stearate, zinc stearate, copper stearate, cobalt stearate, magnesium stearate and praseodymium stearate.

[0016] The dimethyl carbonate-butylene glycol-organic acid copolymer is one of a dimethyl carbonate-butylene glycol-furandicarboxylic acid copolymer or a dimethyl carbonate-butylene glycol-cyclohexanedicarboxylic acid copolymer, and has a number average molecular weight of 30,000 to 70,000.

[0017] The inorganic nano material is one of nano calcium carbonate, nano talc, nano silicon dioxide and nano hydrotalcite.

[0018] The light stabilizer is at least one of 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, methyl p-aminobenzoate, ethyl p-aminobenzoate, butyl p-aminobenzoate and glyceryl p-aminobenzoate.

[0019] The antioxidant is a mixture of a hindered phenol antioxidant and a phosphite antioxidant in a weight ratio of 1:1-2, wherein the models of the hindered phenol antioxidant include 1010, 1076, 1024 and 1520, and the phosphite antioxidant includes trimethyl phosphate, triethyl phosphate, tributyl phosphate, triphenyl phosphate, triethyl phosphite, triphenyl phosphite and antioxidant 168.

[0020] The high barrier biodegradable film of the present invention uses PBAT, polypropylene carbonate, dimethyl carbonate-butylene glycol-organic acid copolymers, etc., which are all biodegradable materials and will not cause white pollution to the environment. By configuring the premix, the compatibility of PBAT and dimethyl carbonate-butylene glycol-organic acid copolymers is improved in the premix configuration stage, reducing the problem of poor compatibility of PBAT, polypropylene carbonate, and dimethyl carbonate-butylene glycol-organic acid copolymers caused by mixing all materials at one time. The barrier properties are further improved by adding inorganic nanomaterials, while improving the shortcomings of the PBAT melt adhesion mold. The biodegradable film of the present invention has simple processing conditions, and can be processed using film blowing equipment, has good barrier properties, and has good development prospects. DETAILED DESCRIPTION

[0021] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work should belong to the protection scope of the present invention.

[0022] Test method

[0023] The testing instruments in the following embodiments are respectively a moisture permeability tester, Permatram-W3 / 61, produced by MOCON Corporation of the United States; and an oxygen permeability tester, Model 8001, produced by Illinois Corporation of the United States.

[0024] Example 1

[0025] A high barrier biodegradable film, the raw materials for preparation include:

[0026] PBAT, molecular weight 100,000, 80 parts.

[0027] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0028] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 50,000, 8 parts.

[0029] Polyethylene glycol, 6 parts;

[0030] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0031] Nano-montmorillonite, 5 parts;

[0032] Zinc stearate, 0.5 part;

[0033] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0034] Antioxidant 168, 0.5 parts, Antioxidant 1010, 0.5 parts.

[0035] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0036] S1: 40 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, and 0.5 parts of zinc stearate were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0037] S2: 40 parts of PBAT, 8 parts of dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0038] S3: Premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.5 parts of antioxidant 168, and 0.5 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain a mixture.

[0039] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0040] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0041] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0042] Example 2

[0043] A high barrier biodegradable film, the raw materials for preparation include:

[0044] PBAT, molecular weight 100,000, 80 parts.

[0045] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0046] Dimethyl carbonate-butanediol-cyclohexanedicarboxylic acid copolymer, molecular weight 50,000, 8 parts.

[0047] Polyethylene glycol, 6 parts;

[0048] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts

[0049] Nano-montmorillonite, 5 parts;

[0050] Zinc stearate, 0.5 part;

[0051] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0052] Antioxidant 168, 0.5 parts, Antioxidant 1010, 0.5 parts.

[0053] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0054] S1: 40 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0055] S2: 40 parts of PBAT, 8 parts of dimethyl carbonate-butylene glycol-cyclohexanedicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0056] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0057] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0058] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0059] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0060] Example 3

[0061] A high barrier biodegradable film, specifically comprising:

[0062] PBAT, molecular weight 100,000, 80 parts.

[0063] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0064] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 50,000, 5 parts.

[0065] Polyethylene glycol, 6 parts;

[0066] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0067] Nano-montmorillonite, 5 parts;

[0068] Zinc stearate, 0.5 part;

[0069] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0070] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0071] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0072] S1: 40 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0073] S2: 40 parts of PBAT, 5 parts of dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0074] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0075] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0076] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0077] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0078] Example 4

[0079] A high barrier biodegradable film, specifically comprising:

[0080] PBAT, molecular weight 100,000, 100 parts.

[0081] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0082] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 50,000, 8 parts.

[0083] Polyethylene glycol, 6 parts;

[0084] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0085] Nano-montmorillonite, 5 parts;

[0086] Zinc stearate, 0.5 part;

[0087] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0088] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0089] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0090] S1: 50 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0091] S2: 50 parts of PBAT, 8 parts of dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0092] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0093] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0094] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0095] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0096] Example 5

[0097] A high barrier biodegradable film, specifically comprising:

[0098] PBAT, molecular weight 100,000, 80 parts.

[0099] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0100] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 70,000, 5 parts.

[0101] Polyethylene glycol, 6 parts;

[0102] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0103] Nano-montmorillonite, 5 parts;

[0104] Zinc stearate, 0.5 part;

[0105] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0106] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0107] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0108] S1: 40 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0109] S2: 40 parts of PBAT, 5 parts of dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0110] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0111] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0112] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0113] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0114] Example 6

[0115] A high barrier biodegradable film, specifically comprising:

[0116] PBAT, molecular weight 100,000, 80 parts.

[0117] Polypropylene carbonate, molecular weight 100,000, 4 parts.

[0118] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 50,000, 8 parts.

[0119] Polyethylene glycol, 6 parts;

[0120] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0121] Nano-montmorillonite, 5 parts;

[0122] Zinc stearate, 0.5 part;

[0123] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0124] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0125] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0126] S1: Add 40 parts of PBAT, 4 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 1000 rpm; mix for 10 minutes to obtain premix A.

[0127] S2: 40 parts of PBAT, 8 parts of dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0128] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0129] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0130] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0131] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0132] Example 7

[0133] A high barrier biodegradable film, specifically comprising:

[0134] PBAT, molecular weight 100,000, 100 parts.

[0135] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0136] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 50,000, 8 parts.

[0137] Polyethylene glycol, 6 parts;

[0138] 5-Hydroxymethyl-2-furancarboxylic acid, 1 part;

[0139] Nano-montmorillonite, 5 parts;

[0140] Zinc stearate, 0.5 part;

[0141] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0142] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0143] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0144] S1: 50 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0145] S2: 50 parts of PBAT, 8 parts of dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, 3 parts of epoxidized soybean oil, 1 part of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0146] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0147] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0148] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0149] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0150] Example 8

[0151] A high barrier biodegradable film, specifically comprising:

[0152] PBAT, molecular weight 100,000, 80 parts.

[0153] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0154] Dimethyl carbonate-butanediol-cyclohexanedicarboxylic acid copolymer, molecular weight 70,000, 8 parts.

[0155] Polyethylene glycol, 6 parts;

[0156] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0157] Nano-montmorillonite, 5 parts;

[0158] Zinc stearate, 0.5 part;

[0159] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0160] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0161] According to the above raw material components and the preparation method provided by the present invention, a high barrier biodegradable film is prepared.

[0162] S1: 40 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0163] S2: 40 parts of PBAT, 8 parts of dimethyl carbonate-butylene glycol-cyclohexanedicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0164] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0165] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0166] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0167] The obtained high barrier biodegradable film was tested for various properties, and the results are shown in Table 1.

[0168] Comparative Example 1

[0169] A biodegradable film, specifically comprising:

[0170] PBAT, molecular weight 100,000, 80 parts.

[0171] Polypropylene carbonate, molecular weight 100,000, 6 parts.

[0172] Polyethylene glycol, 6 parts;

[0173] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0174] Nano-montmorillonite, 5 parts;

[0175] Zinc stearate, 0.5 part;

[0176] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0177] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0178] According to the above raw material components and the preparation method provided by the present invention, a biodegradable film is prepared.

[0179] S1: 40 parts of PBAT, 6 parts of polypropylene carbonate, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0180] S2: 40 parts of PBAT, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0181] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0182] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain biodegradable particles.

[0183] S5: drying the above biodegradable particles at 60°C for 4 hours, and then adding them into a film blowing machine at 160-240°C to obtain a biodegradable film.

[0184] The obtained biodegradable film was tested for various properties, and the results are shown in Table 1.

[0185] Comparative Example 2

[0186] A biodegradable film, specifically comprising:

[0187] PBAT, molecular weight 100,000, 80 parts.

[0188] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 50,000, 8 parts.

[0189] Polyethylene glycol, 6 parts;

[0190] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0191] Nano-montmorillonite, 5 parts;

[0192] Zinc stearate, 0.5 part;

[0193] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0194] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0195] According to the above raw material components and the preparation method provided by the present invention, a biodegradable film is prepared.

[0196] S1: 40 parts of PBAT, 3 parts of polyethylene glycol, 0.5 parts of zinc stearate, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 1000 rpm; mixed for 10 minutes to obtain premix A.

[0197] S2: 40 parts of PBAT, 8 parts of dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, 3 parts of polyethylene glycol, 2 parts of 5-hydroxymethyl-2-furancarboxylic acid, 0.15 parts of antioxidant 168, and 0.15 parts of antioxidant 1010 were added into a high-speed mixer, and the speed of the high-speed mixer was set to 800 rpm; mixed for 5 minutes to obtain premix B.

[0198] S3: Add premix A, premix B and 5 parts of nano-montmorillonite, 0.3 parts of 2-hydroxy-4-methoxybenzophenone, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010 into a high-speed mixer, and set the speed of the high-speed mixer to 800 rpm; mix for 5 minutes to obtain a mixture.

[0199] S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain a biodegradable granule with high barrier properties.

[0200] S5: drying the above-mentioned high barrier biodegradable particles at 60° C. for 4 hours, and then adding them into a film blowing machine at 160-240° C. to obtain a high barrier biodegradable film.

[0201] Various performance tests were performed on the obtained high barrier biodegradable film, and the results are shown in Table 1. Various performance tests were performed on the obtained biodegradable film, and the results are shown in Table 1.

[0202] Comparative Example 3

[0203] A biodegradable film, specifically comprising:

[0204] PBAT, molecular weight 100,000, 80 parts.

[0205] Dimethyl carbonate-butanediol-furandicarboxylic acid copolymer, molecular weight 50,000, 8 parts.

[0206] Polyethylene glycol, 6 parts;

[0207] 5-Hydroxymethyl-2-furancarboxylic acid, 2 parts;

[0208] Nano-montmorillonite, 5 parts;

[0209] Zinc stearate, 0.5 part;

[0210] 2-Hydroxy-4-methoxybenzophenone, 0.3 parts;

[0211] Antioxidant 168, 0.5 parts, antioxidant 1010, 0.5 parts.

[0212] According to the above raw material components and the preparation method provided by the present invention, a biodegradable film is prepared.

[0213] All materials are added into a high-speed mixer at one time, and the speed of the high-speed mixer is set to 1000 rpm; mix for 10 minutes to obtain a mixture. The above-mentioned uniformly mixed mixture is added into a twin-screw extruder, and granulated at 160-240°C to obtain a biodegradable granule. The above-mentioned biodegradable granules are dried at 60°C for 4 hours, and then added into a 160-240°C film blowing machine for processing to obtain a biodegradable film.

[0214] The obtained biodegradable film was tested for various properties, and the results are shown in Table 1.

[0215] Table 1 Performance test results of Examples 1-8 and Comparative Examples 1-3 (thickness of the film is 15 μm)

[0216]

[0217] From the comparison between Comparative Example 1 and Example 1, it can be seen that when the raw material lacks dimethyl carbonate-butylene glycol-furandicarboxylic acid copolymer, the water vapor permeation rate increases from 18 g / (m 2 •24h) rises to 641 g / (m 2 •24h), oxygen permeability 6.2cm 3 / (m 2 •24h•0.1MPa) rises to 346cm 3 / (m 2 •24h•0.1MPa). This shows that dimethyl carbonate-butylene glycol-furan dicarboxylic acid copolymer can significantly improve the barrier properties after being evenly dispersed with PBAT because of its high segment rigidity, small free volume, and cyclic structure. Compared with adding dimethyl carbonate-butylene glycol-furan dicarboxylic acid copolymer and polypropylene carbonate at the same time, when dimethyl carbonate-butylene glycol-furan dicarboxylic acid copolymer is not added and only polypropylene carbonate is added, the barrier effect is poor.

[0218] From the comparison between Comparative Example 2 and Example 1, it can be seen that when the raw material lacks polypropylene carbonate, the water vapor transmission rate increases from 18 g / (m 2 •24h) rise 485g / (m 2 •24h), oxygen permeability 6.2cm 3 / (m 2 •24h•0.1MPa) rises to 279cm 3 / (m 2•24h•0.1MPa). This shows that although the barrier property is improved by adding only dimethyl carbonate-butylene glycol-furan dicarboxylic acid copolymer, it is far less than that by adding dimethyl carbonate-butylene glycol-furan dicarboxylic acid copolymer and polypropylene carbonate at the same time.

[0219] By comparing Comparative Example 3 with Example 1, it can be seen that after all the biodegradable film components are added to the high-speed mixer at one time, the poor compatibility of polypropylene carbonate and dimethyl carbonate-butylene glycol-furandicarboxylic acid copolymer in PBAT has not been completely improved, resulting in a significant improvement in the barrier properties after film formation, but the improvement is far less than that of the premix method.

Claims

1. A method for preparing a high barrier biodegradable film, characterized in that: The steps include: S1: Add 30-55 parts of PBAT, 1-10 parts of polypropylene carbonate, 2-5 parts of plasticizer, 0.1-1 part of heat stabilizer and 0.1-1 part of antioxidant into a high-speed mixer, set the speed of the high-speed mixer to 800-1500 rpm, mix for 5-20 minutes, and obtain premix A; S2: 30 to 55 parts of PBAT, 1 to 10 parts of dimethyl carbonate-butylene glycol-organic acid copolymer, 2 to 5 parts of plasticizer, 0.5 to 3 parts of 5-hydroxymethyl-2-furancarboxylic acid and 0.1 to 1 part of antioxidant are added into a high-speed mixer, and the speed of the high-speed mixer is set to 800 to 1500 rpm to obtain premix B; The dimethyl carbonate-butylene glycol-organic acid copolymer is one of a dimethyl carbonate-butylene glycol-furandicarboxylic acid copolymer or a dimethyl carbonate-butylene glycol-cyclohexanedicarboxylic acid copolymer, and has a number average molecular weight of 30,000 to 70,000; S3: adding premix A, premix B and 2 to 8 parts of inorganic nanomaterials, 0.1 to 1 part of light stabilizer and 0.1 to 1 part of antioxidant into a high-speed mixer, setting the speed of the high-speed mixer to 800 to 1500 rpm to obtain a mixture; the inorganic nanomaterial is one of nano calcium carbonate, nano talc, nano silicon dioxide and nano hydrotalcite; S4: adding the uniformly mixed mixture into a twin-screw extruder and granulating at 160-240° C. to obtain high-barrier biodegradable granules; S5: Dry the high barrier biodegradable particles at 50°C-80°C for 2-8 hours, and then process them in a film blowing machine at 160°C-240°C to obtain a high barrier biodegradable film.

2. The method for preparing a high barrier biodegradable film according to claim 1, characterized in that: The number average molecular weight of the PBAT is 50,000 to 150,000.

3. The method for preparing a high barrier biodegradable film according to claim 1, characterized in that: The number average molecular weight of the polypropylene carbonate is 80,000 to 150,000.

4. The method for preparing a high barrier biodegradable film according to claim 1, characterized in that: The plasticizer is at least one of polyethylene glycol, triethyl citrate, acetyl tri-n-butyl citrate, epoxy soybean oil, and triacetin.

5. The method for preparing a high barrier biodegradable film according to claim 1, characterized in that: The heat stabilizer is at least one of barium stearate, calcium stearate, zinc stearate, copper stearate, cobalt stearate, magnesium stearate and praseodymium stearate.

6. The method for preparing a high barrier biodegradable film according to claim 1, characterized in that: The light stabilizer is at least one of 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, methyl p-aminobenzoate, ethyl p-aminobenzoate, butyl p-aminobenzoate and glyceryl p-aminobenzoate.

7. The method for preparing a high barrier biodegradable film according to claim 1, characterized in that: The antioxidant is a mixture of a hindered phenol antioxidant and a phosphite antioxidant in a weight ratio of 1:1-2, wherein the models of the hindered phenol antioxidant include 1010, 1076, 1024 and 1520, and the phosphite antioxidant includes trimethyl phosphate, triethyl phosphate, tributyl phosphate, triphenyl phosphate, triethyl phosphite, triphenyl phosphite and antioxidant 168.

Citation Information

Cited By

  • High-stiffness high-barrier biodegradable packaging material and preparation method thereof

    CN120310208A