A protective film and a co-extrusion process for preparing the same
By forming grooves on the substrate layer of the lithium battery protective film, the problems of poor exhaust gas and insufficient bonding performance in the prior art are solved, and the surface of the lithium battery is flat and safe. Performance improvement.
Patent Information
- Application Number
- CN202211474408.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-23
AI Technical Summary
The existing lithium battery protective film has poor exhaust gas during bonding, resulting in uneven surface of the battery cell, insufficient bonding performance, easy warping, and unable to effectively prevent damage from impact and drop of lithium batteries.
A plurality of isolated grooves are formed on the surface of the substrate layer, and adhesive units are embedded to increase the bonding area. A gas discharge is achieved by using the non-adhesive exhaust passage of the substrate layer surface to ensure smooth fit and not easy to warp.
It improves the adhesion and exhaust effect of the lithium battery protective film, ensures that the surface of the lithium battery is flat and fits, reduces safety risks, and improves the safety performance of the lithium battery.
Smart Images

Figure CN115851153B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of protective films, and in particular, relates to a protective film and a co-extrusion process for preparing the same. Background Art
[0002] Lithium batteries are widely used in electronic products, electric vehicles, energy storage base stations, etc., due to their high operating voltage, long cycle life, high power tolerance, and no memory effect. They are considered to be one of the most promising chemical power sources. When power lithium-ion batteries are used in the field of new energy vehicles, due to the characteristics of high-speed movement, severe vibration, high-temperature operation, and rapid charging and discharging when the car is driving, the power batteries are subject to potential dangers such as collision, puncture, short connection, falling, immersion in water, and fire when in use.
[0003] In order to avoid potential safety hazards caused by impact, scratches, and falls, a protective film is applied to the surface of lithium batteries to prevent damage to the batteries. However, during the process of applying the protective film, poor exhaust can easily lead to uneven surfaces on the battery cells. Even if the PET protective film has an exhaust channel set by glue dots or grids, the glue dots or grids are mostly formed on the PET substrate by coating, and the contact area is flat. The composite is not strong, and it is easy to leave residual glue when peeling off. There is also debonding at high temperatures, which leads to warping, and the battery cells cannot be protected.
[0004] In view of the above-mentioned defects of existing products, it is necessary to explore a protective film that can be used for square batteries, has good exhaust effect, good adhesion performance, and is not easy to warp. Summary of the invention
[0005] The object of the present invention is to provide a protective film and a co-extrusion process for preparing the same, which can ensure that the adhesive force of the protective film is sufficient to fix the battery, and has good exhaust effect, meets the appearance requirements of a smooth surface after being bonded to a square battery, and is not easy to warp.
[0006] According to a first aspect of the present invention, a protective film is provided, comprising a substrate layer and a plurality of adhesive units, wherein a plurality of mutually isolated grooves are formed on the surface of the substrate layer, the adhesive units are embedded in the grooves, and the adhesive units fill the grooves so that the plurality of adhesive units are distributed on the surface of the substrate layer at intervals from each other.
[0007] The protective film provided by the present invention has a special structure that can increase the composite area between the adhesive unit and the substrate layer, thereby increasing the bonding force between the adhesive unit and the substrate layer. When the protective film fully coated with the adhesive layer is pasted to the battery during use, air is easily present between the adhesive layer and the surface of the battery to be pasted due to poor exhaust. When the protective film of the present invention is pasted to the battery, the gas can be discharged along the non-sticky substrate surface between the adhesive units where no adhesive unit is set, so that the protective film can better fit the surface of the lithium battery, and the laminating effect is good, it is not easy to warp, and the appearance is good.
[0008] Preferably, in the depth direction of the groove, the surface of the adhesive unit that is not bonded with the groove serves as the adhesive surface of the adhesive unit, and the adhesive surface of the adhesive unit is flush with the notch of the groove.
[0009] Thus, the adhesive unit and the substrate in the protective film together form a continuous and flat surface without any concave or convex. When the protective film is used, there is less space between the protective film and the battery, which is conducive to the close fitting and tight wrapping of the lithium battery. The flat surface will not affect the exhaust performance of the protective film. There is no sticky substrate layer to separate the adhesive unit, and the air can be exhausted by being squeezed to the substrate layer on the adhesive surface. The use of the protective film of the present invention can reduce the possibility of potential safety hazards in the battery and improve the safety performance of the lithium battery.
[0010] Preferably, the spacing distance between adjacent adhesive units is M, the width of the adhesive surface of the adhesive unit is N, and 1≤N / M≤4.
[0011] When the N / M ratio is within the above range, the adhesion and exhaust functions of the protective film are maintained within an appropriate range, which can provide sufficient adhesion to ensure that the protective film and the battery fit tightly, and can ensure that the protective film can smoothly discharge bubbles and fill the gaps.
[0012] Preferably, M=1-13.5 mm, N=1-54 mm.
[0013] The value range of M and N can meet the sizes of most batteries on the market, has a wide range of uses, and is highly feasible for mass production.
[0014] Preferably, the maximum thickness of the substrate layer is denoted as H, the maximum depth of the groove is denoted as H1, and 0.08
[0015] By limiting the ratio of the maximum depth of the groove to the maximum thickness of the substrate layer within the range of 0.08 to 1, the area of the composite surface of the adhesive unit and the substrate layer can be sufficiently large, further improving the adhesion between the adhesive unit and the substrate layer and improving the reliability of the protective film.
[0016] Preferably, the maximum thickness H of the substrate layer is 30 to 120 μm.
[0017] When the maximum thickness of the substrate layer, i.e. the total thickness of the protective film, is 30 to 120 μm, sufficient space can be provided for the embedding of the adhesive unit, and the protective film can be prevented from being too thick, thereby reducing the space occupied by the protective film and improving the energy density of the module.
[0018] Preferably, the maximum depth H1 of the groove is 10-50 μm.
[0019] The maximum depth H1 of the groove is the maximum thickness of the adhesive unit. When the adhesive unit is 10 to 50 μm, sufficient adhesive force can be ensured.
[0020] Preferably, when H is in the range of 30 to 80 μm, the protective film further comprises a continuous adhesive layer and an isolation layer sequentially stacked on the back side of the groove opening surface of the substrate layer, and the material of the continuous adhesive layer is the same as that of the adhesive unit.
[0021] Preferably, the raw material of the isolation layer is at least one of PET, PBT and PC.
[0022] Preferably, the raw materials forming the adhesive unit include, by weight, 38-47% styrene-isoprene-styrene block copolymer (SIS block copolymer), 39-48% tackifying resin, 19-24% cyclohexane oil and 0.5-2.5% antioxidant.
[0023] The adhesive unit made using this adhesive has excellent bonding properties and stronger bonding force, which can ensure that the protective film can play its own bonding role and avoid the battery falling off due to insufficient bonding force of the adhesive layer itself during use and falling.
[0024] Preferably, the raw materials of the adhesive unit are 40% SIS block copolymer, 40% tackifying resin, 19% naphthenic oil and 1% antioxidant. Thus, the adhesive unit can maintain high plasticity, and the adhesive layer has strong adhesion, further improving the appearance smoothness of the protective film after lamination.
[0025] Preferably, the tackifying resin is selected from at least one of C5 hydrogenated petroleum resin, C9 petroleum resin, rosin resin and terpene resin.
[0026] Preferably, the antioxidant is a mixture of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and tris(2,4-di-tert-butylphenyl)phosphite, and the weight ratio of the antioxidant to pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and tris(2,4-di-tert-butylphenyl)phosphite is 2:1.
[0027] Preferably, the raw material of the substrate layer includes PET resin.
[0028] Preferably, the raw material of the substrate layer further includes an anti-hydrolysis agent.
[0029] Preferably, the raw material of the substrate layer further includes a pigment.
[0030] Preferably, the pigment includes at least one of ultramarine, iron blue, cobalt blue, phenol blue, lake blue and indigo.
[0031] Preferably, the amount of the anti-hydrolysis agent added is 1-19%, which is a percentage of the mass of the raw material of the substrate layer. Further, the amount of the anti-hydrolysis agent added can be 3%, 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19%.
[0032] Preferably, the PET resin is selected from at least one of film-grade PET resin, bottle-grade PET resin or fiber-grade PET resin.
[0033] Preferably, the PET resin is a PET resin produced by DuPont of the United States with a brand number of 936CSNC011.
[0034] Preferably, the anti-hydrolysis agent includes monomeric carbodiimide and polymeric carbodiimide.
[0035] Preferably, the anti-hydrolysis agent is produced by Shanghai Langyi Functional Materials Co., Ltd., with the brand name Anti-hydrolysis agent.
[0036] According to another aspect of the present invention, a coextrusion process for preparing the above-mentioned protective film is provided, comprising the following steps: allowing a base film melt and a first adhesive layer melt to enter a coextrusion die, merge, and extrude into a film through a coextrusion die head of the coextrusion die, wherein the base film melt is fed into the coextrusion die in a continuous feeding manner, and the first adhesive layer melt is fed into the coextrusion die in an intermittent feeding manner, and the interval distance M between adjacent adhesive units arranged in the protective film and / or the width N of the adhesive surface of the adhesive unit are regulated by controlling the frequency of the intermittent feeding of the first adhesive layer melt; wherein the base film melt refers to a molten slurry used to form a substrate layer, and the first adhesive layer melt refers to a molten slurry used to form an adhesive unit, and the base film melt and the first adhesive layer melt do not melt each other; in the depth direction of the groove, the surface of the adhesive unit that is not compounded with the groove is used as the adhesive surface of the adhesive unit.
[0037] The present invention uses a co-extrusion process to prepare the above-mentioned protective film. The process flow is simple, the prepared protective film has good uniformity and consistency, and the co-extrusion molding cycle is short, the energy consumption is low, the process is simple, the operation is simple, and the interlayer adhesion between the substrate layer and the adhesive unit is good. This solution adjusts the feeding method of the base film melt and the first adhesive layer melt, and can produce the above-mentioned protective film with strong adhesion, good exhaust effect, smooth appearance after bonding, and not easy to warp through a simple process.
[0038] Preferably, the raw materials of the substrate layer are mixed evenly and then kneaded in a single-screw or twin-screw extruder to obtain a base film melt; the raw materials of the first adhesive layer are mixed evenly and then kneaded in a single-screw or twin-screw extruder to obtain a first adhesive layer melt.
[0039] Preferably, the temperature of the co-extrusion die for extruding the film is 215-240°C, specifically 215°C, 220°C, 225°C, 230°C, 235°C, 240°C.
[0040] When the co-extrusion die extrusion film forming temperature is 215-240°C, the viscosity of the substrate layer raw material fluid is similar to that of the first adhesive layer raw material fluid, which makes it easy to control the extrusion rate and reduce the defective rate. In addition, the first adhesive layer and the substrate layer in the obtained protective film have good adhesion and are not easy to fall off.
[0041] Preferably, the temperature of the first adhesive layer melt is 200-240°C, specifically 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C.
[0042] Preferably, the temperature of the base film melt is 215-280°C, specifically 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, 265°C, 270°C, 275°C, 280°C.
[0043] Preferably, the coextrusion process also includes the following steps: melt-kneading the evenly mixed second adhesive layer raw materials and isolation layer raw materials to obtain a continuous adhesive layer melt and an isolation layer melt respectively, then co-extrude the isolation layer melt, the continuous adhesive layer melt, the base film melt and the first adhesive layer melt through a four-layer coextrusion die to obtain a coextrusion blank, then cast film and perform unidirectional and / or bidirectional stretching as needed to finally obtain a protective film; the self-adhesive surface of the protective film thus obtained is sequentially an adhesive unit, a substrate layer, a continuous adhesive layer and an isolation layer, wherein the second adhesive layer melt forms a continuous adhesive layer, the substrate layer includes a first surface and a second surface arranged opposite to each other, the first surface forms a plurality of mutually isolated grooves, the adhesive unit is embedded in the grooves, and the continuous adhesive layer is compounded with the second surface of the substrate layer.
[0044] The continuous adhesive layer and isolation layer on the second side are also made by co-extrusion process, which does not require additional equipment cost, has simple process, low processing cost, energy saving, and wide product application. At the same time, the co-extrusion process produces less three waste substances, does not use organic solvents, and has less environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 Schematic diagram of the cross section of the protective film prepared in Examples 1 and 2;
[0046] Figure 2 is a schematic cross-sectional view of the protective film prepared in Comparative Example 1;
[0047] Figure 3 Schematic diagram of the cross section of the protective film prepared in Comparative Example 2;
[0048] Figure 4 is a schematic cross-sectional view of the protective film prepared in Example 3;
[0049] Figure 5 A schematic diagram of the adhesive surface of the protective film prepared in the present invention;
[0050] In the above drawings, the corresponding relationship of each figure mark is: 1. adhesive unit, 2. substrate layer, 3. continuous adhesive layer; 4. isolation layer; 5. exhaust channel; N. width of the adhesive surface of the adhesive unit, M. spacing distance between adjacent adhesive units. DETAILED DESCRIPTION
[0051] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0052] Example 1
[0053] The raw material formula for preparing the adhesive unit in this embodiment is as follows: 40 parts of SIS block copolymer, 40 parts of terpene resin, 19 parts of cyclohexane oil, 0.67 parts of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and 0.33 parts of tris(2,4-di-tert-butylphenyl)phosphite; the raw material formula for preparing the substrate layer is as follows: 22 parts of anti-hydrolysis agent, 176 parts of film-grade PET resin, 0.9 parts of phthalocyanine blue, 0.9 parts of titanium dioxide, and 0.2 parts of carbon black.
[0054] Prepare the materials according to the raw material formula of the adhesive unit and the substrate layer used in this embodiment, mix the required materials evenly according to the formula ratio, and prepare the protective film according to the following steps:
[0055] S1. Loading: The substrate layer raw materials and adhesive unit raw materials prepared and mixed according to the above formula ratio are respectively placed into different loading ports of the co-extrusion equipment. The adhesive unit raw materials are intermittently fed, and the substrate layer raw materials are continuously fed.
[0056] Among them, a baffle that can move forward and backward periodically is provided below the raw material feeding port of the gluing unit. When the baffle moves forward to the maximum extent, it can completely block the raw material feeding port of the gluing unit; when the baffle moves forward to the minimum extent, the raw material feeding port of the gluing unit is completely unobstructed. When the baffle completely blocks the raw material feeding port of the gluing unit, it will pause, and the pause time t1 is 1×10 -2 s. The baffle starts to move from the place where the feeding port of the gluing unit raw material machine is completely blocked, moves to the place where the feeding port of the gluing unit raw material machine is completely unblocked, and then moves back to the original position and pauses. This is a baffle movement cycle, and it repeats in this way. The cycle time t is 3.5×10 -2 As the baffle plate moves back and forth periodically, the feeding amount of the gluing unit also changes periodically, realizing intermittent feeding.
[0057] S2, melt plasticization treatment: melt and mix the raw materials of the substrate layer to form a base film melt, the melting temperature of the base film melt is 220°C, and the first screw is rotated to realize the conveyance of the base film melt, and the speed of the first screw is 300r / min; melt and mix the raw materials of the adhesive unit to form a first adhesive layer melt, the melting temperature of the first adhesive layer melt is 240°C, and the second screw is rotated to realize the conveyance of the base film melt, and the speed of the second screw is 300r / min;
[0058] S3, converging: the base film melt and the first adhesive layer melt are extruded into a first melt through a co-extrusion film head to form a co-extrusion blank and a film-like object. The co-extrusion temperature of the first melt is 230° C. and the film outlet speed v is 800 mm / s.
[0059] S4, film casting: the film is cast onto a steadily rotating chilled roller, cooled and shaped to obtain a protective film.
[0060] In particular, the thickness of the protective film is measured, and the movement of the baffle in S1 is controlled according to the measured thickness of the adhesive unit.
[0061] When the thickness of the adhesive unit in the protective film is detected to be 1±0.2 μm, the baffle is controlled to move to completely cover the feed inlet and pause, and the pause time t is 1×10 -2 s, and then the baffle continues to move periodically; when the thickness of the adhesive unit is detected to be greater than 40μm, the baffle is controlled to move forward, reducing the amount of adhesive unit feeding, making the thickness of the adhesive unit smaller. If the thickness is detected to be continuously greater than 40μm, check whether the baffle is damaged.
[0062] The protective film structure obtained in this embodiment is as follows Figure 1As shown, the surface of the substrate layer 2 forms a plurality of grooves isolated from each other, and the adhesive unit 1 is embedded in the groove, and the adhesive unit 1 fills the groove, so that the plurality of adhesive units 1 are distributed on the surface of the substrate layer at intervals. In the depth direction of the groove, the surface of the adhesive unit 1 that is not compounded with the groove is used as the adhesive surface of the adhesive unit 1, and the adhesive surface of the adhesive unit 1 is flush with the notch of the groove. In the protective film prepared in this embodiment, the spacing distance M between adjacent adhesive units 1 is 8 mm, the width N of the adhesive surface of the adhesive unit 1 is 20 mm, the maximum depth H1 of the groove is 40 μm, and the thickness of the protective film, that is, the maximum thickness H of the substrate layer, is 110 μm.
[0063] Comparative Example 1
[0064] This comparative example refers to the method for preparing a protective film provided in Example 1 to prepare a protective film. The difference between this comparative example and Example 1 is that the extrusion method of the first adhesive layer melt is continuous extrusion, specifically, the lower baffle of the adhesive unit raw material feeding port is kept in a state of minimum forward movement, that is, the adhesive unit raw material feeding port is completely unobstructed during the preparation process, so that the first adhesive layer melt is extruded into a continuous adhesive layer blank. The remaining raw materials and preparation methods are strictly consistent with those in Example 1, so that H and H1 in the prepared protective film are strictly consistent with those in Example 1. The prepared protective film is as follows Figure 2 As shown, the adhesive unit 1 is compounded on the surface of the substrate layer 2 , the compound surface of the two is a flat plane, and the adhesive unit 1 is raised relative to the surface of the substrate layer 2 .
[0065] Comparative Example 2
[0066] The substrate layer and adhesive unit formula used in Example 1 were prepared, and the PET substrate layer was extruded by a single-layer extrusion method, so that the thickness of the substrate layer was strictly consistent with H in Example 1. In addition, the first adhesive layer raw material and the solvent were mixed into a uniform glue according to the formula ratio, and the glue was applied on one side of the substrate layer by intermittent coating. The glue was applied by intermittent coating to form a plurality of adhesive units 1 arranged at intervals on the surface of the substrate layer 2, and the glue applied on the surface of the substrate layer 2 was dried to form an adhesive layer with a thickness strictly consistent with H1 in Example 1. In the length direction of the protective film, the spacing M between adjacent adhesive units 1 in the protective film and the width N of the adhesive surface of the adhesive unit 1 were strictly consistent with those in Example 1.
[0067] The protective film prepared in this comparative example is as follows Figure 3 As shown, a plurality of adhesive units 1 arranged at intervals are formed on the surface of the substrate layer 2 , and the adhesive units 1 are raised relative to the surface of the substrate layer 2 .
[0068] Example 2
[0069] Experimental Group 2-1
[0070] This experimental group prepared a protective film by referring to the method for preparing a protective film provided in Example 1. The difference between this experimental group and Example 1 is that the spacing distance M of the adhesive unit 1 in the prepared protective film is 10 mm, specifically, the baffle pause time t1 in the preparation method is changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that N, H1 and H in the prepared protective film are strictly consistent with those in Example 1.
[0071] Experimental group 2-2
[0072] This experimental group prepared a protective film by referring to the method for preparing a protective film provided in Example 1. The difference between this experimental group and Example 1 is that the spacing distance M of the adhesive unit 1 in the prepared protective film is 20 mm, specifically, the baffle pause time t1 in the preparation method is changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that N, H1 and H in the prepared protective film are strictly consistent with those in Example 1.
[0073] Experimental Group 2-3
[0074] This experimental group prepared a protective film by referring to the method for preparing a protective film provided in Example 1. The difference between this experimental group and Example 1 is that the adhesive surface width N of the adhesive unit 1 in the prepared protective film is 32 mm, specifically, the periodic motion time t of the baffle in the preparation method is changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that H1 and H in the prepared protective film are strictly consistent with those in Example 1.
[0075] Experimental Groups 2-4
[0076] This experimental group refers to the method for preparing a protective film provided in Example 1 to prepare a protective film. The difference between this experimental group and Example 1 is that the adhesive surface width N of the adhesive unit 1 in the prepared protective film is 40 mm, specifically, the periodic motion time t of the baffle in the preparation method is changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that H1 and H in the prepared protective film are strictly consistent with those in Example 1.
[0077] Experimental Groups 2-5
[0078] This experimental group refers to the method for preparing a protective film provided in Example 1 to prepare a protective film. The difference between this experimental group and Example 1 is that the maximum thickness H1 of the adjacent adhesive units 1 in the prepared protective film is 20 μm, specifically, the speed of the first screw in the preparation method is changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that N, M and H in the prepared protective film are strictly consistent with those in Example 1.
[0079] Experimental Groups 2-6
[0080] This experimental group prepared a protective film by referring to the method for preparing a protective film provided in Example 1. The difference between this experimental group and Example 1 is that the maximum thickness H1 of the adjacent adhesive units 1 in the prepared protective film is 5 μm, specifically, the speed of the first screw in the preparation method is changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that N, M and H in the prepared protective film are strictly consistent with those in Example 1.
[0081] Experimental Groups 2-7
[0082] This experimental group refers to the method for preparing a protective film provided in Example 1 to prepare a protective film. The difference between this experimental group and Example 1 is that the maximum thickness H1 of the adjacent adhesive units 1 in the prepared protective film is 30 μm, specifically, the speed of the first screw in the preparation method is changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that N and M in the prepared protective film are strictly consistent with those in Example 1.
[0083] Experimental Groups 2-8
[0084] This experimental group prepared a protective film by referring to the method for preparing a protective film provided in Example 1. The difference between this experimental group and Example 1 is that the maximum thickness H1 of the adjacent adhesive units 1 in the prepared protective film is 27 μm, and the maximum thickness H of the substrate layer is 30 μm. Specifically, the rotation speeds of the first screw and the second screw in the preparation method are changed. The remaining raw materials, preparation method and process parameters are strictly consistent with those in Example 1, so that N and M in the prepared protective film are strictly consistent with those in Example 1.
[0085] Test Example 1
[0086] 1. Test objects: The protective films prepared in Example 1, Comparative Example 1, Comparative Example 2, and Experimental Group 2 were used as test objects.
[0087] 2. Test items
[0088] The test objects of this test example are the protective films prepared in Examples 1 to 2 and Comparative Examples 1 to 2, and the following tests are performed on the test objects:
[0089] (1) Adhesion test: At room temperature, the protective film adhered to the aluminum shell of the lithium battery pack was repeatedly laminated and peeled off five times, and the amount of residual adhesive on the aluminum shell was observed;
[0090] (2) Cohesion test: The protective film is attached to a mirror-finished stainless steel plate with an area of 1 inch. 2 , apply a 1KG weight along the bonding direction, and observe the displacement of the protective film after 48 hours;
[0091] (3) Warping resistance test: The prepared protective film was wrapped around the aluminum shell and folded at a distance of 4 mm from the edge of the protective film. After 48 hours, the protective film was observed to see if there was any warping at the corners and folded edges.
[0092] (4) Insulation test: The surface resistance of the protective film at 1000 V and the breakdown voltage under AC and DC conditions were measured;
[0093] (5) Flatness test: The prepared protective film was wrapped on the surface of 100 aluminum shells, and the number of aluminum shells with uneven surfaces was recorded.
[0094] 3. Test results: The product dimensions of the test objects and their calculation results are shown in Table 1, and the test results are shown in Table 2.
[0095] According to the test results in Table 2, the protective films of Example 1 and Example 2 have higher comprehensive performance than those of Comparative Example 1 and Comparative Example 2. Figure 1 As shown, the surface of the substrate layer 2 forms a plurality of mutually isolated grooves, and the adhesive unit 1 is embedded in the grooves, and the adhesive unit 1 fills the grooves, so that the plurality of adhesive units 1 are distributed on the surface of the substrate layer 2 at intervals. This special structure can increase the composite area between the adhesive unit 1 and the substrate layer 2, thereby increasing the bonding force between the adhesive unit 1 and the substrate layer 2. The protective film needs to be bent and twisted during use to completely wrap the lithium battery, and during the bending process of the commercially available protective film, the air between the protective film and the battery shell is not discharged smoothly. Figure 5 As shown, the air between the protective film of the present invention and the battery shell can be discharged through the exhaust channel 5 composed of the non-sticky substrate layer 2 on the adhesive surface, so that the protective film can better fit the surface of the lithium battery with good fitting effect and good appearance.
[0096] like Figure 2 As shown, the adhesive layer in the protective film of comparative example 1 is a continuous adhesive layer. In Table 2, the adhesion, cohesion and insulation of comparative example 1 are similar to those of the protective film of Example 1, which means that the adhesive performance of the protective film using the spaced adhesive unit in Example 1 is similar to that of the protective film using the continuous adhesive layer. However, the air exhaust performance of the protective film of comparative example 1 is poor. From the warpage resistance test, it can be seen that the protective film of comparative example 1 warps at the folded edge and the corner. From the flatness test, it can be seen that the protective film of comparative example 1 is not smooth in air exhaust during lamination. 8 out of 100 samples have flatness problems.
[0097] Comparing Comparative Example 2 with Example 1, Comparative Example 2 uses a coating process, and the adhesion and cohesion of the protective film produced are worse than those of Example 1, but the warpage resistance, insulation and flatness are similar to those of the protective film of Example 1. The reasons are speculated to be the following three aspects: first, the protective film produced by the co-extrusion process has good uniformity and consistency; second, Figure 3 As shown, the adhesive unit 1 in the protective film of comparative example 2 is compounded on the surface of the substrate layer 2, and the adhesive unit 1 is raised relative to the surface of the substrate layer 2, while the adhesive unit 1 in the protective film of embodiment 1 is embedded in the surface of the substrate layer 2, and the contact surface between the substrate layer 2 and the adhesive unit 1 is large, and the interlayer adhesion is good; thirdly, because the adhesive surface of the protective film of embodiment 1 is a flat plane, there is less space between the protective film and the battery when the protective film of embodiment 1 is used, which is conducive to the close fitting and tight wrapping of the lithium battery, and the exhaust performance of embodiment 1 is equivalent to that of comparative example 2, because the air in the protective films of embodiment 1 and comparative example 2 can be smoothly exhausted along the exhaust channel 5 formed by the non-adhesive substrate on the adhesive surface. In summary of the above three reasons, the adhesion and cohesion of embodiment 1 are greater, and the overall effect is better than the performance of the protective film with conventional exhaust adhesive layer.
[0098] From the data of Example 1 and experimental groups 2-1 to 2-4 in Table 2, it can be seen that the performance of experimental groups 2-1 to 2-3 is better than that of Example 1, and experimental group 2-4 has problems of warping and low flatness, which means that when the ratio of N / M satisfies 1≤N / M≤4, and M=1~13.5mm, N=1~54mm, the adhesion, cohesion, warping resistance, insulation and flatness of the protective film are all maintained within the appropriate range, which can provide sufficient adhesion to make the protective film fit tightly with the battery, and can ensure that the protective film can smoothly discharge air and fill the gap. Among them, all the performance indicators of Example 1 are the best, indicating that when N is 20mm and M is 8mm in the protective film, its comprehensive performance is the best. The N / M ratio of the protective film in experimental group 2-4 is 5. In the warping resistance test, the protective film warped at the folded edge; in the flatness test, 4 out of 100 samples had flatness problems.
[0099] Comparing Example 1 with experimental groups 2-5 to 2-8, the performance of experimental groups 2-5, 2-7, and 2-8 is better than that of Example 1, indicating that when H1 is 10 to 50 μm, H is 30 to 120 μm, and 0.08 < H1 / H < 1, it is possible to ensure that the area of the composite surface of the adhesive unit 1 and the substrate layer 2 is large enough, improve the adhesion between the adhesive unit 1 and the substrate layer 2, and improve the reliability of the protective film. Among them, the comprehensive performance in Example 1 is the best, indicating that when H1 is 40 μm and H is 110 μm in the protective film, its comprehensive performance is the best. The H1 of the protective film in experimental group 2-6 was 5μm, and the thickness of adhesive unit 1 was too small. In the cohesion test, the protective film was displaced by 7mm. In the flatness test, 7 out of 100 samples had uneven surfaces. In the warping resistance test, the protective film warped at the corners and edges, indicating that the flexibility and adhesion of the protective film in experimental group 2-6 were poor and could not tightly wrap the battery.
[0100] Table 1. Product dimensions and calculation results of the test objects in Test Example 1
[0101] Group N(mm) M(mm) N / M(au) <![CDATA[H1(μm)]]> H(μm) <![CDATA[H1 / H(a.u.)]]> Example 1 20 8 2.5 40 110 0.36 Comparative Example 1 / 0 / 40 110 0.36 Comparative Example 2 20 8 2.5 40 110 0.36 Experimental Group 2-1 20 10 2 40 110 0.36 Experimental group 2-2 20 20 1 40 110 0.36 Experimental Group 2-3 32 8 4 40 110 0.36 Experimental Groups 2-4 40 8 5 40 110 0.36 Experimental Groups 2-5 20 8 2.5 20 110 0.18 Experimental Groups 2-6 20 8 2.5 5 110 0.05 Experimental Groups 2-7 20 8 2.5 30 110 0.27 Experimental Groups 2-8 20 8 2.5 27 30 0.90
[0102] Table 2. Performance test results of the test objects in test case 1
[0103]
[0104]
[0105] Example 3
[0106] This experimental group prepared a protective film by referring to the method for preparing a protective film provided in Example 1. Figure 4 , which is different from Example 1 in that H=50μm, and further comprises the following steps on the basis of Example 1: melt-kneading the uniformly mixed second adhesive layer raw material and the isolation layer raw material to obtain a continuous adhesive layer melt and an isolation layer melt respectively, and then co-extrude the isolation layer melt, the continuous adhesive layer melt, the base film melt and the first adhesive layer melt through a four-layer co-extrusion die to obtain a co-extruded blank, and then cast film and perform uniaxial and / or biaxial stretching as required to finally obtain a protective film; the protective film thus obtained is as follows Figure 4 As shown, the self-adhesive surface comprises an adhesive unit 1, a substrate layer 2, a continuous adhesive layer 3 and an isolation layer 4 in sequence, wherein the second adhesive layer melt forms the continuous adhesive layer 3, the substrate layer 2 comprises a first surface and a second surface arranged opposite to each other, the first surface is provided with a plurality of grooves isolated from each other, the adhesive unit 2 is embedded in the groove, and the continuous adhesive layer 3 is compounded with the second surface of the substrate layer 1.
[0107] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A protective film, characterized in that: The protective film comprises a substrate layer and a plurality of adhesive units, a plurality of mutually isolated grooves are formed on the surface of the substrate layer, the adhesive units are embedded in the grooves, and the adhesive units fill the grooves, so that the plurality of adhesive units are distributed on the surface of the substrate layer at intervals; the raw material of the substrate layer comprises PET resin; the maximum thickness of the substrate layer is H, the maximum depth of the groove is H1, 0.08<H1 / H<0.9; In the depth direction of the groove, the surface of the adhesive unit that is not compounded with the groove serves as the adhesive surface of the adhesive unit, and the adhesive surface of the adhesive unit is flush with the notch of the groove; the spacing distance between the adjacent adhesive units is M, and the width of the adhesive surface of the adhesive unit is N, 1≤N / M≤4.
2. The protective film according to claim 1, characterized in that: The M=1-13.5 mm, and the N=1-54 mm.
3. The protective film according to claim 1, characterized in that: The maximum thickness H of the substrate layer is 30 to 120 μm.
4. The protective film according to claim 1 or 3, characterized in that: When H is in the range of 30-80 μm, the protective film further comprises a continuous adhesive layer and an isolation layer sequentially stacked on the back side of the groove opening surface of the substrate layer, and the material of the continuous adhesive layer is the same as the material of the adhesive unit.
5. The protective film according to claim 1, characterized in that: The raw materials forming the adhesive unit include, by weight, 38-47% of styrene-isoprene-styrene block copolymer (SIS block copolymer), 39-48% of tackifying resin, 19-24% of naphthenic oil and 0.5-2.5% of antioxidant.
6. A co-extrusion process for preparing the protective film according to any one of claims 1 to 5, characterized in that: The following operations are included: The base film melt and the first adhesive layer melt are combined and extruded through a co-extrusion die head of a co-extrusion die to form a film, wherein the base film melt is fed into the co-extrusion die in a continuous feeding manner, and the first adhesive layer melt is fed into the co-extrusion die in an intermittent feeding manner, and the interval distance M between the adjacent adhesive units in the protective film and / or the width N of the adhesive surface of the adhesive unit are regulated by controlling the frequency of the intermittent feeding of the first adhesive layer melt; The base film melt refers to the molten slurry used to form the substrate layer, and the first adhesive layer melt refers to the molten slurry used to form the adhesive unit. The base film melt and the first adhesive layer melt are not soluble in each other.
7. The coextrusion process according to claim 6, characterized in that: The following steps are also included: After the uniformly mixed second adhesive layer raw materials and isolation layer raw materials are melt-kneaded, a continuous adhesive layer melt and an isolation layer melt are obtained respectively; then the isolation layer melt, the continuous adhesive layer melt, the base film melt and the first adhesive layer melt are co-extruded through a four-layer co-extrusion die to obtain a co-extruded composite blank; then, a film is cast and unidirectionally and / or bidirectionally stretched as needed to finally obtain a protective film; the self-adhesive surfaces of the protective film thus obtained are an adhesive unit, a substrate layer, a continuous adhesive layer and an isolation layer in sequence, wherein the second adhesive layer melt forms the continuous adhesive layer, the substrate layer includes a first surface and a second surface arranged opposite to each other, the first surface forms a plurality of mutually isolated grooves, the adhesive unit is embedded in the groove, and the continuous adhesive layer is composited with the second surface of the substrate layer.