A thermal resistance long-life red room temperature phosphorescent material and its application
Through the design of amorphous polymers, combined with the copolymerization of pyrene groups and sodium p-styrene sulfonate, a thermal resistance long-life red room temperature phosphorescent material is formed, which solves the problem of phosphorescence performance degradation in high temperature environments and achieves phosphorescence at high temperatures. Launch and anti-counterfeiting applications, reducing costs and processing difficulty.
Patent Information
- Application Number
- CN202211459288.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-17
AI Technical Summary
The phosphorescent performance of existing pure organic room-temperature phosphorescent materials decreases in high-temperature environments, making it difficult to achieve long-life red phosphorescent emission, which limits their application in high-temperature environments.
Using amorphous polymers, a water-soluble polymer is formed by synthesizing functionalized phosphors and copolymerizing with sodium p-styrene sulfonate. The red phosphorescence emission potential of the pyrene group and the intermolecular π-π interaction are used to suppress triplet excitons. Non-radiative transition, a thermal resistance long-life red room temperature phosphorescent material was prepared.
It achieves the ability to maintain phosphorescence emission at room temperature and high temperature. The material is easily soluble in water and has low cost. It overcomes the difficulty in preparing crystal materials and the brittleness problem, and provides prospects for anti-counterfeiting and data encryption applications in high-temperature environments.
Smart Images

Figure CN115851264B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to organic room temperature phosphorescent luminescent materials, and particularly relates to a thermal resistance type long-life red room temperature phosphorescent material and application thereof. Background Art
[0002] Pure organic room temperature phosphorescent materials have the advantages of low cost, good biocompatibility, and easy structural modification, which have attracted great attention. These unique advantages enable them to be applied in many fields such as organic light-emitting diodes, bioimaging, information encryption, and anti-counterfeiting. However, the weak spin-orbit coupling and fast non-radiative decay of triplet excitons lead to inefficient system crosstalk (ISC), making it difficult to achieve long-lived phosphorescent emission. Generally speaking, the generation of organic phosphorescence involves two key processes: (1) increasing the energy from the lowest excited singlet state (S1) to the excited triplet state (T n ) and the intersystem crossing (ISC) efficiency from the lowest excited triplet state (T1) to the ground state (S0). This can be effectively achieved by enhancing spin-orbit coupling or reducing the energy gap between the singlet and triplet states. (2) Inhibiting the non-radiative transition process from the lowest excited triplet state to the ground state. However, due to the violent molecular thermal motion (vibration, collision, diffusion motion, etc.) and the quenching effect of oxygen, it is difficult to observe organic phosphorescence at room temperature. In recent years, domestic and foreign researchers have developed a series of high-efficiency organic long afterglow materials using strategies such as crystal engineering, constructing host-guest systems to form hydrogen bond networks, polymer matrix doping, and aggregated state induced emission.
[0003] Although there are continuous reports that RTP systems have ultra-long lifetimes from microseconds (ms) to seconds (s), there are few reports on red afterglow in pure polymer systems, and materials with high RTP efficiency are still quite limited. More importantly, the phosphorescence is quenched due to the significant non-radiative transitions (violent vibrational relaxation) of triplet excitons at high temperatures. This thermal quenching effect is an obstacle to high luminescence efficiency and greatly limits the applicability of long afterglow materials in high temperature environments. At present, there are only a few studies on zero thermal quenching phosphorescent materials, and most of them are inorganic materials. Pure organic long afterglow materials have not yet been reported.
[0004] Therefore, how to develop a polymer long-life luminescent material that still has good phosphorescent properties under high temperature conditions is a technical problem to be solved by those skilled in the art. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a thermal resistance type long-life red room temperature phosphorescent material to solve the problem that the current long-life organic room temperature phosphorescent material cannot be used in a high temperature environment.
[0006] The invention also provides a method for preparing the heat-resistance type long-life red room-temperature phosphorescent material.
[0007] Furthermore, the present invention also provides the application of the above-mentioned thermal resistance type red room temperature phosphorescent material in data encryption and anti-counterfeiting.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0009] A thermal resistance type long-life red room temperature phosphorescent material, characterized by comprising a polymer with the following structure:
[0010]
[0011] Furthermore, the thermal resistance type long-life red room temperature phosphorescent material is obtained by the following preparation method:
[0012] S1. Synthesis of functionalized phosphors:
[0013]
[0014] The mass ratio of 1-hydroxypyrene to 4-chloromethylstyrene is 0.7 to 1.5, and the reaction time is 10 to 48 hours.
[0015] S2. Synthesis of copolymer of functionalized phosphor and sodium p-styrene sulfonate:
[0016]
[0017] The molar ratio of the functionalized phosphor to sodium p-styrene sulfonate is 1:100 to 1:1500, and the reaction time is 24 to 72 hours.
[0018] The present invention also provides the application of the thermal resistance type long-life red room temperature phosphorescent material, which is used in the fields of data encryption and anti-counterfeiting under different temperature conditions, and the different temperatures include 77-400K.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention uses amorphous polymers to prepare the world's first long-life red room temperature phosphorescent material with thermal resistance. The polymer long afterglow material of the present invention can achieve phosphorescent emission at room temperature and high temperature at the same time, has a high degree of concealment, is easy to use, and is easy to identify, thereby achieving a higher level of anti-counterfeiting function, and has a good application prospect in the fields of organic optoelectronic materials and anti-counterfeiting encryption. In addition, the polymer long afterglow material is easily soluble in water and can be easily processed into various shapes.
[0021] 2. The present invention functionalizes a universal small molecule chromophore and then performs free radical polymerization with sodium p-styrene sulfonate. The obtained water-soluble polymer long afterglow material produces blue fluorescence visible to the naked eye under 365nm ultraviolet light. When the excitation light source is turned off, a red afterglow visible to the naked eye can be produced, and the afterglow duration can reach 2s. Increasing the temperature will not cause quenching of the phosphorescence emission of the material, and a red afterglow visible to the naked eye can still be produced at a high temperature of 400K.
[0022] 3. The composition of the polymer long afterglow material of the present invention is simple. Unlike inorganic phosphorescent materials, it does not require rare elements and the cost is greatly reduced. In addition, the present invention overcomes the shortcomings of difficult preparation of crystalline materials, high brittleness, poor stability, and easy phase separation and difficult processing of small molecule host-guest doped long afterglow materials.
[0023] 4. The preparation method of the present invention has the advantages of easy control, simple operation, low production cost, and provides a new strategy for designing thermal resistance type room temperature phosphorescent materials. It also has good application prospects in the fields of anti-counterfeiting encryption in high temperature environments. It is easy to realize industrial production, providing new theoretical guidance and technical support for the simple and efficient industrialization of thermal resistance type polymer room temperature phosphorescent materials, and also enriching the preparation method of pure polymer room temperature phosphorescent materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is the H NMR spectrum of 1-hydroxypyrene functionalized phosphor;
[0025] Figure 2 is the infrared spectrum of 1-hydroxypyrene functionalized phosphor;
[0026] Figure 3 is the infrared spectrum of the polymer;
[0027] Figure 4 This is the afterglow photo of the polymer under the excitation of 365nm ultraviolet light in room temperature atmosphere;
[0028] Figure 5 This is the phosphorescence spectrum of the polymer under 365nm ultraviolet light excitation in room temperature and atmospheric environment;
[0029] Figure 6 This is the phosphorescence lifetime decay curve of the polymer under 365nm ultraviolet light excitation in room temperature and atmospheric environment;
[0030] Figure 7 The phosphorescence spectrum of the polymer under the excitation of 365nm ultraviolet lamp at the temperature of 80K-280K;
[0031] Figure 8 The phosphorescence lifetime decay curve of the polymer under 365nm ultraviolet light excitation at temperatures of 80K-280K;
[0032] Fig. 9 The phosphorescence spectrum of the polymer under 365nm ultraviolet light excitation at a temperature of 300K-400K;
[0033] Fig.10 The phosphorescence lifetime decay curve of the polymer under 365nm ultraviolet light excitation at a temperature of 300K-400K;
[0034] Fig.11 This is an afterglow photograph of a polymer excited by a 365nm ultraviolet lamp at a temperature of 300K-400K. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with embodiments.
[0036] 1. A thermal resistance type long-life red room temperature phosphorescent material, comprising a polymer having the following structure:
[0037]
[0038] The present invention has found that the structure contains pyrene groups and pyrene molecules have the potential for red phosphorescence emission; in addition, the large conjugated structure of pyrene can form a strong intermolecular π-π interaction, which can provide a rigid environment for triplet excitons and inhibit their non-radiative transitions; due to the rigidity of the polymer structure, the polymer chain moves slowly in a high-temperature environment, reducing the vibrational relaxation of the triplet excitons, allowing it to still have phosphorescence emission in an environment above room temperature.
[0039] 2. A method for preparing a thermal resistance type long-life red room temperature phosphorescent material, comprising the following steps:
[0040] S1. Synthesis of functionalized phosphors:
[0041]
[0042] The mass ratio of 1-hydroxypyrene to 4-chloromethylstyrene is 0.7 to 1.5, and the reaction time is 10 to 48 hours.
[0043] S2. Synthesis of copolymer of functionalized phosphor and sodium p-styrene sulfonate:
[0044]
[0045] The molar ratio of the functionalized phosphor to sodium p-styrene sulfonate is 1:100 to 1:1500, and the reaction time is 24 to 72 hours.
[0046] 3. The prepared polymer was irradiated with ultraviolet light at different temperatures. After removing the excitation light source, the afterglow phenomenon at different temperatures was observed, proving that the polymer is a thermal resistance-type long-life red room-temperature phosphorescent material with the function of data storage and anti-counterfeiting applications in high-temperature environments.
[0047] Example 1
[0048] A method for preparing a heat-resistance type long-life red room temperature phosphorescent material (a polymer long afterglow material) comprises the following steps:
[0049] (1) Synthesis of 1-hydroxypyrene functionalized phosphors
[0050] 2.18 g 1-hydroxypyrene, 1.12 g potassium hydroxide, and 30 mL tetrahydrofuran were added to a three-necked flask, stirred at 70°C for 30 minutes under condensation reflux, and then 2.11 mL 4-chloromethylstyrene was added dropwise with a syringe, and the mixture was reacted at 70°C for 45 hours under condensation reflux. After the reaction, the mixture was rinsed and filtered three times with water and methanol, and vacuum dried at 65°C for 24 hours to obtain a yellow powder product.
[0051] Through nuclear magnetic resonance hydrogen spectrum and infrared spectrum detection, it can be seen that the yellow powder product has the following structure:
[0052]
[0053] like Figure 1 As shown in the hydrogen nuclear magnetic resonance spectrum, there are 8 groups of signals in the figure, and the integrated intensity ratio is 1:7:1:4:1:1:2:1, which is consistent with the structure of the 1-hydroxypyrene functionalized phosphor small molecule. The chemical shifts of each group are also consistent, indicating that the synthesized yellow powder product is our expected product.
[0054] like Figure 2 As shown in the infrared spectrum, the peak at 2922cm-1 is the stretching vibration peak of the -CH2- bond, the absorption peaks at 1627cm-1, 1597cm-1, 1506cm-1, and 1457cm-1 are the characteristic peaks of the stretching vibration of the benzene ring skeleton, the sawtooth-shaped double frequency absorption of 1700cm-1-2000cm-1 is the overtone absorption of the bending vibration of the CH out-of-plane and C=C in-plane on the benzene ring, 1254cm-1 is the characteristic peak of the in-plane vibration of the CH of the benzene ring, 1016cm-1 is the characteristic peak of the stretching vibration of CO, 907cm-1 and 990cm-1 appear the characteristic peaks of the out-of-plane deformation vibration of the CH of -CH=CH2, and 827cm-1 is the characteristic peak of the deformation vibration of the CH of the para-substituted benzene ring. The above shows that the 1-hydroxypyrene functionalized phosphor has been successfully synthesized.
[0055] (2) Preparation of thermal resistance long-life red room temperature phosphorescent materials
[0056] 0.0167 g of the product obtained in step (1), 4.12 g of sodium p-styrene sulfonate, 41.3 mg of 2,2-azobisisobutyronitrile, and 30 mL of ultra-dry dimethyl sulfoxide are added to a polymerization tube; vacuum evacuation and argon gas flow are repeated, and the reaction is carried out at 65° C. for 48 hours to obtain a viscous liquid; then, the liquid is poured into a large amount of ethanol for reprecipitation, and finally vacuum dried at 80° C. for 48 hours to obtain a copolymer of 1-hydroxypyrene functionalized phosphor and sodium p-styrene sulfonate with a molar ratio of 1:400.
[0057] Through infrared spectrum detection, it can be seen that the copolymer has the following structure:
[0058]
[0059] like Figure 3 As shown in the infrared spectrum, the stretching vibration peak of the -CH2- bond is at 2924cm-1, and the characteristic peaks of the sulfonic acid group are at 1179cm-1, 1126cm-1, 670cm-1, and 577cm-1, indicating that the copolymer of 1-hydroxypyrene functionalized phosphor and sodium p-styrene sulfonate has been successfully synthesized.
[0060] Example 2
[0061] The prepared polymer is irradiated with ultraviolet light at different temperatures, and afterglow phenomena at different temperatures can be observed after the excitation light source is removed.
[0062] Under room temperature and atmospheric environment, the polymer obtained in Example 1 was irradiated with a 365 nm ultraviolet lamp. Figure 4 As shown, it has blue fluorescence emission under 365nm ultraviolet excitation, and red afterglow can be clearly observed after removing the excitation light source, and the afterglow lasts for 2 seconds.
[0063] The polymer obtained in Example 1 was excited by a 365 nm ultraviolet lamp at room temperature and the phosphorescence emission spectrum was obtained as follows: Figure 5 The phosphorescence lifetime decay curve is as follows: Figure 6 .Depend on Figure 5 and Figure 6 It can be seen that the phosphorescence emission peaks of the polymer are at 614 nm and 676 nm, and the phosphorescence lifetime at 614 nm is 222.70 ms.
[0064] The polymer was excited with a 365nm ultraviolet lamp at a temperature of 80 to 280K, and the phosphorescence spectrum results at a temperature of 80 to 280K were obtained as follows Figure 7 The phosphorescence lifetime decay curve is as follows: Figure 8 It can be seen that the phosphorescence intensity of the polymer gradually decreases as the temperature increases, which shows that the polymer belongs to a room temperature phosphorescent material and has no thermally activated delayed fluorescence.
[0065] The polymer was excited with a 365nm ultraviolet lamp at a temperature of 300-400K, and the phosphorescence spectrum results at a temperature of 300-400K were obtained as follows: Fig. 9 The phosphorescence lifetime decay curve is as follows: Fig.10 It can be seen that the phosphorescence intensity of the polymer gradually decreases with increasing temperature, and at a high temperature of 400K, the phosphorescence lifetime is 16.70ms.
[0066] Fig.11 The afterglow photos of the present invention after being irradiated with a 365nm ultraviolet lamp at different temperatures are shown. It can be seen that the afterglow of the present invention can still be observed when the temperature reaches 400K.
[0067] Example 3-5 shows long-life red phosphorescence after excitation by 365nm UV lamp
[0068]
[0069] In summary, the present invention functionalizes a universal small molecule chromophore, and then performs free radical polymerization with sodium p-styrene sulfonate. The obtained water-soluble polymer long afterglow material shows long-life red phosphorescence after being excited by a 365nm ultraviolet lamp. More importantly, the phosphorescence of the polymer has obvious thermal resistance characteristics, and the red afterglow is still visible to the naked eye when the temperature reaches 400K. The preparation method of the polymer material is simple to operate and has low production cost. It provides a new strategy for designing thermal resistance room temperature phosphorescent materials, and has good application prospects in the fields of anti-counterfeiting encryption in high temperature environments.
[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A thermal resistance long-life red room temperature phosphorescent material, characterized in that: The copolymer comprises a functionalized phosphor and sodium p-styrene sulfonate; the functionalized phosphor has a structural formula as shown in formula (1): The structural formula of the sodium p-styrene sulfonate is shown in formula (2): The molar ratio of the functionalized phosphor to sodium p-styrene sulfonate is 1:100 to 1:1500.
2. A method for preparing a thermal resistance type long-life red room temperature phosphorescent material, characterized in that: The steps include: S1. Synthesis of functionalized phosphors: The mass ratio of 1-hydroxypyrene to 4-chloromethylstyrene is 0.7 to 1.5, and the reaction time is 10 to 48 hours; S2. Synthesis of copolymer of functionalized phosphor and sodium p-styrene sulfonate: The molar ratio of the functionalized phosphor to sodium p-styrene sulfonate is 1:100 to 1:1500, and the reaction time is 24 to 72 hours.
3. Application of a thermal resistance type long-life red room temperature phosphorescent material, characterized in that: The phosphorescent material described in claim 1 is used in the fields of data encryption and anti-counterfeiting under different temperature conditions.
4. The use of the thermal resistance type long-life red room temperature phosphorescent material according to claim 3, characterized in that: The temperature range is 77-400K.