A composite fiber with island-bridge structure and preparation method thereof

By introducing island bridge structure and phase difference twisting force into polyamide fibers, combined with stretching and heat setting technology, the problem of insufficient curling elasticity of polyamide fibers is solved, and its three-dimensional curling performance is significantly improved, so that it can replace it Spandex fiber.

CN115852523BActive Publication Date: 2024-11-26GUANGDONG XINHUI MEIDA NYLON
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211623130.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-11-26
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The initial modulus of polyamide composite fibers is relatively low, resulting in insufficient curling elasticity and cannot completely replace spandex fibers. It is difficult for the prior art to significantly improve its three-dimensional curling effect.

Method used

The composite fibers with island bridge structures are used to generate twisting forces through the differences in viscosity or heat shrinkage properties of island structure fibers and bridge structure fibers, forming a flat island bridge structure. Combined with stretching and heat setting technology, the curling elasticity of the fibers is improved.

Benefits of technology

The curling elasticity of polyamide composite fibers is significantly improved, so that it can reach or exceed the performance of polyester composite fibers, and can effectively replace spandex fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852523B_ABST
    Figure CN115852523B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of textile technology, and specifically discloses a composite fiber with an island-bridge structure and a preparation method thereof. The composite fiber includes two island structure fibers and one bridge structure fiber. The bridge structure fiber is arranged between the two island structure fibers to connect the two island structure fibers together and form a flat island-bridge structure with large ends and a small middle. Both the island structure fiber and the bridge structure fiber are polyamide fibers. The viscosity or thermal shrinkage rate of the island structure fiber is greater than that of the bridge structure fiber. The island structure fiber of the composite fiber of the present invention adopts a polyamide fiber with a large molecular weight and good rigidity; the bridge structure fiber adopts a polyamide fiber with a small molecular weight and good flexibility. After the island-bridge structure composite fiber is stretched and heat-set, due to the difference in the performance of the two fibers, a twisting force will be generated inside the fiber, so that the composite fiber has good three-dimensional curling performance and elasticity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textile technology, and in particular relates to a composite fiber with an island-bridge structure and a preparation method thereof. Background Art

[0002] At present, there are two main processing methods for the curly elasticity of chemical fibers. One is to make the fibers curl by mechanical processing to obtain curly elastic fibers, such as chemical fiber stretch yarn (DTY) and air-deformed yarn (ATY). The elasticity of this fiber is weak and easily attenuated. After being woven into fabrics, the elasticity is insufficient. A certain proportion of spandex fiber must be mixed to achieve a good elastic effect. However, spandex fiber does not absorb color, making the fabric difficult to dye. Another three-dimensional curly elastic fiber is made by a composite spinning method, such as polyester (PET / PTT) elastic composite fiber. This fiber is produced by a parallel composite method and has good curly elasticity. It can be used in fabrics to replace spandex. At present, this composite fiber has also been widely used in the market.

[0003] Polyamide (PA) composite curly elastic fibers have not been well developed. The main reason is that the initial modulus of polyamide fibers is relatively low, resulting in low curly elasticity of polyamide parallel composite fibers, which cannot completely replace spandex fibers and therefore cannot be widely used.

[0004] Therefore, there is an urgent need to develop a polyamide-based elastic composite fiber with good three-dimensional curling effect and elasticity to replace spandex. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a composite fiber with an island-bridge structure and a preparation method thereof, wherein the composite fiber has an island-bridge structure, and the island structure fiber and the bridge structure fiber are two polyamide fibers with large differences in viscosity or thermal shrinkage performance. The performance difference between the two fibers is utilized to generate a twisting force inside the composite fiber, thereby improving the curling elasticity of the composite fiber.

[0006] In order to solve the above technical problems, the first aspect of the present invention provides a composite fiber, which includes two island structure fibers and one bridge structure fiber. The bridge structure fiber is arranged between the two island structure fibers to connect the two island structure fibers together to form a flat island bridge structure with large ends and a small middle; the island structure fibers and the bridge structure fibers are both polyamide fibers; the relative viscosity or thermal shrinkage rate of the island structure fibers is greater than that of the bridge structure fibers.

[0007] Specifically, the composite fiber of the present invention has an island-bridge structure, in which two island structure fibers are connected together by a bridge structure fiber, and the island structure fiber adopts a polyamide fiber with a large molecular weight and good rigidity, and the bridge structure fiber adopts a polyamide fiber with a small molecular weight and good flexibility. After the island-bridge structure composite fiber is stretched and heat-set, due to the difference in the performance of the two fibers, a twisting force will be generated inside the fiber. The island-bridge structure of the present invention is flat, which is more conducive to the twisting of the fiber to form a spiral curled state than the skin-core structure and the parallel structure. The combined effect of multiple factors can significantly improve the curling elasticity of the composite fiber.

[0008] At the same time, the cross section of the composite fiber of the present invention is an island-bridge structure with large ends and a small middle, wherein the heat shrinkage rate of the island structure fibers at the two ends is higher, while the heat shrinkage rate of the bridge structure fibers in the middle slender part is lower. This structure provides a greater possibility for the two fiber materials to be twisted due to heat shrinkage, thereby making the composite fiber have better curling performance and better three-dimensional curling elasticity. The cross section of ordinary composite fibers is generally in an inverted "8" shape. The two fiber materials in this structure are more closely combined. Even if there is a certain difference in heat shrinkage rate between the two fiber materials, the maximum twisting of the fiber is limited due to the too close combination, which will affect the improvement of the fiber's elasticity.

[0009] As a further improvement of the above solution, the relative viscosity of the island structure fibers is 0.5-1.5 higher than the relative viscosity of the bridge structure fibers.

[0010] As a further improvement of the above solution, the thermal shrinkage rate of the island structure fibers is 1.5-3.0 times the thermal shrinkage rate of the bridge structure fibers.

[0011] Specifically, when the two fiber raw materials used in the composite fiber of the present invention are of the same type (such as low-viscosity PA6 / high-viscosity PA6), it is necessary to ensure that the relative viscosity of the island structure fiber is 0.5-1.5 higher than the relative viscosity of the bridge structure fiber; if the two fiber raw materials are of different types (such as PA6 / PA66), it is necessary to ensure that the relative viscosity of the island structure fiber is 0.5-1.5 higher than the relative viscosity of the bridge structure fiber or the thermal shrinkage rate is 1.5-3.0 times the thermal shrinkage rate of the bridge structure fiber.

[0012] At the same time, appropriate relative viscosity difference and thermal shrinkage difference are more conducive to the stability of composite fiber production, thereby ensuring product quality. Polyamide fibers with too small relative viscosity difference or thermal shrinkage difference will produce composite fibers with poor curl elasticity; while polyamide fibers with too large relative viscosity difference or thermal shrinkage difference will easily produce fiber twisting prematurely during composite fiber production, resulting in the formation of elbow fibers at the spinneret outlet, which will cause the composite fibers to produce hairy fibers.

[0013] As a further improvement of the above solution, the island structure fiber includes any one of PA6, PA66, PA56, and COPA; and the bridge structure fiber includes PA6.

[0014] Specifically, the composite fiber of the present invention is composed of two fibers, one fiber includes PA6, and the other fiber includes any one of PA6, PA66, PA56, and COPA; wherein: COPA is copolymer nylon, which is copolymerized by multiple dibasic acids and diamines, and its thermal shrinkage rate is more than twice that of ordinary PA6, PA66, and PA56, and has a higher curling shrinkage rate.

[0015] As a further improvement of the above solution, the mass ratio of the island structure fibers to the bridge structure fibers is 25:75 to 75:25.

[0016] Preferably, the mass ratio of the island structure fibers to the bridge structure fibers is 40:60 to 60:40.

[0017] As a further improvement of the above solution, the length of the bridge structure fiber is 1-5 times the diameter of the island structure fiber; the width of the bridge structure fiber is 0.1-0.5 times the diameter of the island structure fiber.

[0018] Specifically, the composite fiber of the present invention is a flat island-bridge structure with large ends and a small middle. The two ends of the cross section of the island-bridge structure are round and the middle is a long strip. By controlling the size relationship between the length of the bridge structure fiber and the diameter of the island structure fiber, and the width of the bridge structure fiber and the diameter of the island structure fiber, it is more conducive to improving the curling elasticity of the composite fiber while ensuring the stability of the product.

[0019] The second aspect of the present invention provides a method for preparing a composite fiber, the method being used to prepare the composite fiber according to the first aspect of the present invention, comprising the following steps:

[0020] (1) melting the raw materials for preparing the island structure fiber and the raw materials for preparing the bridge structure fiber respectively, and then entering the composite spinning assembly through their respective melt pipes. The two fiber melts are respectively ejected through the spinneret holes of the spinneret and then bonded together to form composite primary fibers with an island-bridge structure;

[0021] (2) The composite spun fibers are cooled, bundled, oiled, stretched, heated, shaped, and wound to obtain the composite fibers.

[0022] Preferably, in step (1), the melting temperature of the island structure fiber is 260-320°C.

[0023] Preferably, in step (1), the melting temperature of the bridge structure fiber is 220-265°C.

[0024] Preferably, in step (1), the pressure of the spinning assembly is 13-25 MPa.

[0025] Preferably, in step (2), the cooling is performed by side blowing, the wind speed of the side blowing is 0.25-0.5 m / s, the wind temperature is 18-20° C., and the humidity is 90-95%.

[0026] Preferably, in step (2), the stretching ratio is 1.2-3.0.

[0027] Preferably, in step (2), the heat setting temperature is 100-180°C.

[0028] Preferably, the specific process flow of the preparation method of the composite fiber is as follows:

[0029] (1) Melting stage: under nitrogen protection, the raw materials for preparing the island structure fiber and the raw materials for preparing the bridge structure fiber are respectively added into a screw extruder, melted, and further mixed uniformly under the stirring of the screw;

[0030] (2) Spinning stage: The island structure fiber melt and the bridge structure fiber melt obtained in step (1) enter the spinning box through different melt pipes, and are ejected through different spinneret holes after passing through the spinning assembly and the spinneret plate, wherein the island structure fiber melt is ejected through the circular spinneret hole, and the bridge structure fiber melt is ejected through the flat spinneret hole, and after ejection, every two circular cross-section fibers are connected head to tail with one flat cross-section fiber to form a composite primary fiber with an island-bridge structure;

[0031] (3) Cooling stage: the composite spun fiber obtained in step (2) is uniformly cooled by side blowing at a constant temperature and humidity;

[0032] (4) Bundling and oiling stage: The fiber tows are collected into bundles after cooling, and then oiled through an oil nozzle and a pre-network device to give the tows good lubricity and saturation, reducing friction and dispersion of the tows;

[0033] (5) Stretching stage: In one stretching process, the fiber can be stretched by setting the speed difference between the front and rear drafting rollers, inducing the orientation and crystallization of the two raw material macromolecules inside the composite fiber. Due to the difference in molecular structure and molecular weight of the two raw materials, the two raw materials will inevitably produce different degrees of orientation and crystallization, so that the two raw material macromolecules will produce different shrinkage and rebound. This unequal shrinkage and rebound will make the composite fiber produce a three-dimensional curled shape, and also obtain good elastic recovery;

[0034] (6) Heating and shaping stage: Heating and shaping are carried out simultaneously with stretching. By setting a suitable shaping process (such as temperature), the composite fiber can obtain the best resilience.

[0035] (7) Winding and forming stage: After the composite fiber is stretched and shaped, the properties of the fiber in all aspects are basically stable. Then, the fiber is wound into a regular-shaped coil by a winding device, thus forming the composite fiber with three-dimensional curled polyamide elasticity of the present invention.

[0036] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:

[0037] (1) The composite fiber of the present invention is composed of two island structure fibers connected together by a bridge structure fiber to form a flat island-bridge structure with large ends and a small middle. The island structure fiber is made of polyamide fiber with a large molecular weight and good rigidity, and the bridge structure fiber is made of polyamide fiber with a small molecular weight and good flexibility. After the island-bridge structure composite fiber is stretched and heat-set, due to the difference in the properties of the two fibers, a twisting force will be generated inside the fiber, thereby making the composite fiber have good three-dimensional curling performance and elasticity.

[0038] (2) The composite fiber with an island-bridge structure of the present invention greatly improves the curl elasticity of the polyamide elastic composite fiber, and its elastic index reaches or exceeds that of the polyester (PET / PTT) elastic composite fiber, and can be used to replace spandex fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a schematic cross-sectional view of the composite fiber of the present invention;

[0040] Figure 2 It is a schematic structural diagram of the composite fiber spinneret of the present invention.

[0041] In the figure: 100 - island structure fiber; 200 - bridge structure fiber; 300 - island structure spinneret hole; 400 - bridge structure spinneret hole. DETAILED DESCRIPTION

[0042] The present invention is described in detail below in conjunction with the examples, so that the technical personnel of the relevant technical field can understand the present invention. It is necessary to point out here that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The non-essential improvements and adjustments made to the present invention by the skilled person in the relevant field according to the above invention content should still belong to the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art.

[0043] The cross-sectional schematic diagram of the composite fiber of the present invention is as follows Figure 1As shown, a composite fiber includes two island structure fibers 100 and a bridge structure fiber 200, wherein: the bridge structure fiber 200 is arranged between the two island structure fibers 100, connects the two island structure fibers 100 together, and forms a flat island bridge structure with large ends and small middle. The cross section of the island structure fiber 100 is circular, and the cross section of the bridge structure fiber 200 is flat and long. The length of the bridge structure fiber 200 is 1-5 times the diameter of the island structure fiber 100; the width of the bridge structure fiber 200 is 0.1-0.5 times the diameter of the island structure fiber 100. By controlling the size relationship between the length of the bridge structure fiber and the diameter of the island structure fiber, and the width of the bridge structure fiber and the diameter of the island structure fiber, it is more conducive to improving the curling elasticity of the composite fiber while ensuring the stability of the product.

[0044] The structural schematic diagram of the composite fiber spinneret of the present invention is as follows Figure 2 As shown, the composite fiber needs to use a spinneret in the spinning stage to form a specific composite fiber structure. The spinnerets in the spinneret of the present invention are composed of two island structure spinnerets 300 and one bridge structure spinneret 400. Every two island structure spinnerets 300 and one bridge structure spinneret 400 form a group. There are multiple spinneret groups of such island-bridge combinations in the same spinneret. The island structure spinnerets 300 are circular, and the island structure fiber melt is ejected through the two island structure spinnerets 300 to form two circular cross-section filaments; the bridge structure spinneret 400 is flat and long, and the bridge structure fiber melt is ejected through a bridge structure spinneret 400 to form a flat cross-section filament. The two circular cross-section filaments ejected through the two island structure spinnerets 300 and one bridge structure spinneret 400 are connected head to tail with a flat cross-section filament to form the composite primary fiber with an island-bridge structure of the present invention.

[0045] Example 1

[0046] A composite fiber, composed of two island structure fibers and one bridge structure fiber, wherein the island structure fiber is high-viscosity PA6 (relative viscosity of 3.16), the bridge structure fiber is low-viscosity PA6 (relative viscosity of 2.46), the relative viscosity of the high-viscosity PA6 is 0.7 higher than that of the low-viscosity PA6. The mass ratio of high-viscosity PA6 to low-viscosity PA6 is 50:50.

[0047] A method for preparing a composite fiber comprises the following steps:

[0048] (1) Melting stage: Under nitrogen protection, high-viscosity PA6 and low-viscosity PA6 are added to their respective screw extruders for melting, wherein the screw zone temperature of high-viscosity PA6 is 260-285°C, and the screw zone temperature of low-viscosity PA6 is 220-265°C;

[0049] (2) Spinning stage: The high-viscosity PA6 melt and the low-viscosity PA6 melt obtained in step (1) enter the spinning manifold through different melt pipes, and are ejected through different spinneret holes after passing through the spinning assembly (pressure 15.5 MPa) and the spinneret, wherein the island structure fiber melt is ejected through the circular spray hole, and the bridge structure fiber melt is ejected through the flat hole. After ejection, every two circular cross-section fibers are respectively bonded together with a flat cross-section fiber at both ends of the flat shape to form a composite primary fiber with an island-bridge structure;

[0050] (3) Cooling stage: The composite spun fiber obtained in step (2) is uniformly cooled by side blowing at a constant temperature and humidity, wherein the cooling wind speed is 0.3 m / s, the wind temperature is 20° C., and the humidity is 93%;

[0051] (4) Bundling and oiling stage: The fiber tows are collected into bundles after cooling, and then oiled through an oil nozzle and a pre-network device to give the tows good lubricity and saturation, reducing friction and dispersion of the tows;

[0052] (5) Stretching stage: stretching the fiber obtained in step (4) at a stretching multiple of 1.25 times;

[0053] (6) Heating and setting stage: Heating and setting are carried out simultaneously with stretching, and the temperature of heat setting is 130°C;

[0054] (7) Winding and forming stage: The composite fiber after being stretched and shaped is wound into a regular-shaped coil by a winding device to obtain the composite fiber of this embodiment.

[0055] Example 2

[0056] A composite fiber, consisting of two island structure fibers and one bridge structure fiber, wherein the island structure fiber is PA66 (relative viscosity is 3.11), the bridge structure fiber is PA6 (relative viscosity is 2.46), the relative viscosity of PA66 is 0.65 higher than that of low viscosity PA6, and the mass ratio of PA66 to PA6 is 50:50.

[0057] A method for preparing a composite fiber comprises the following steps:

[0058] (1) Melting stage: under nitrogen protection, PA66 and PA6 are added to their respective screw extruders for melting, wherein the screw zone temperature of PA66 is 270-310°C, and the screw zone temperature of PA6 is 250-265°C;

[0059] (2) Spinning stage: The PA66 melt and PA6 melt obtained in step (1) enter the spinning manifold through different melt pipes, and are ejected through different spinneret holes after passing through the spinning assembly (pressure 16.0 MPa) and the spinneret, wherein the island structure fiber melt is ejected through the circular spinneret hole, and the bridge structure fiber melt is ejected through the flat hole. After ejection, every two circular cross-section fibers are respectively bonded together with a flat cross-section fiber at both ends of the flat shape to form a composite primary fiber with an island-bridge structure;

[0060] (3) Cooling stage: The composite spun fiber obtained in step (2) is uniformly cooled by side blowing at a constant temperature and humidity, wherein the cooling wind speed is 0.3 m / s, the wind temperature is 20° C., and the humidity is 93%;

[0061] (4) Bundling and oiling stage: The fiber tows are collected into bundles after cooling, and then oiled through an oil nozzle and a pre-network device to give the tows good lubricity and saturation, reducing friction and dispersion of the tows;

[0062] (5) Stretching stage: stretching the fiber obtained in step (4) at a stretching multiple of 1.25 times;

[0063] (6) Heating and setting stage: Heating and setting are carried out simultaneously with stretching, and the temperature of heat setting is 160°C;

[0064] (7) Winding and forming stage: The composite fiber after being stretched and shaped is wound into a regular-shaped coil by a winding device to obtain the composite fiber of this embodiment.

[0065] Example 3

[0066] A composite fiber, composed of two island structure fibers and one bridge structure fiber, wherein the island structure fiber is PA56 (boiling water shrinkage is 19.5%), and the bridge structure fiber is PA6 (boiling water shrinkage is 10.5%), the boiling water shrinkage of PA56 is 1.85 times that of PA6, and the mass ratio of PA56 to PA6 is 50:50.

[0067] A method for preparing a composite fiber comprises the following steps:

[0068] (1) Melting stage: under nitrogen protection, PA56 and PA6 are added to their respective screw extruders for melting, wherein the screw zone temperature of PA56 is 260-295°C, and the screw zone temperature of PA6 is 240-265°C;

[0069] (2) Spinning stage: The PA56 melt and the PA6 melt obtained in step (1) are introduced into the spinning manifold through different melt pipes, and then ejected through different spinneret holes after passing through the spinning assembly (pressure 14.5 MPa) and the spinneret, wherein the island structure fiber melt is ejected through the circular spinneret hole, and the bridge structure fiber melt is ejected through the flat hole. After ejection, every two circular cross-section fibers are respectively bonded together with a flat cross-section fiber at both ends of the flat shape to form a composite primary fiber with an island-bridge structure;

[0070] (3) Cooling stage: The composite spun fiber obtained in step (2) is uniformly cooled by side blowing at a constant temperature and humidity, wherein the cooling wind speed is 0.3 m / s, the wind temperature is 20° C., and the humidity is 93%;

[0071] (4) Bundling and oiling stage: The fiber tows are collected into bundles after cooling, and then oiled through an oil nozzle and a pre-network device to give the tows good lubricity and saturation, reducing friction and dispersion of the tows;

[0072] (5) Stretching stage: stretching the fiber obtained in step (4) at a stretching multiple of 1.2 times;

[0073] (6) Heating and setting stage: Heating and setting are carried out simultaneously with stretching, and the temperature of heat setting is 160°C;

[0074] Winding and forming stage: the composite fiber after being stretched and shaped is rolled into a regular-shaped coil by a winding device to obtain the composite fiber of this embodiment.

[0075] Example 4

[0076] A composite fiber, consisting of two island structure fibers and one bridge structure fiber, wherein the island structure fiber is COPA (boiling water shrinkage is 31.5), and the bridge structure fiber is PA6 (boiling water shrinkage is 10.5), the boiling water shrinkage of COPA is 3.0 times that of PA6, and the mass ratio of COPA to PA6 is 50:50.

[0077] A method for preparing a composite fiber comprises the following steps:

[0078] (1) Melting stage: Under nitrogen protection, COPA and PA6 are added to their respective screw extruders for melting, wherein the screw zone temperature of COPA is 270-295°C, and the screw zone temperature of PA6 is 220-265°C, and further mixed under the stirring of the screw;

[0079] (2) Spinning stage: The COPA melt and PA6 melt obtained in step (1) enter the spinning manifold through different melt pipes, and are ejected through different spinneret holes after passing through the spinning assembly (pressure 14.5 MPa) and the spinneret, wherein the island structure fiber melt is ejected through the circular spinneret hole, and the bridge structure fiber melt is ejected through the flat hole. After ejection, every two circular cross-section fibers are respectively bonded together with a flat cross-section fiber at both ends of the flat shape to form a composite primary fiber with an island-bridge structure;

[0080] (3) Cooling stage: The composite spun fiber obtained in step (2) is uniformly cooled by side blowing at a constant temperature and humidity, wherein the cooling wind speed is 0.3 m / s, the wind temperature is 20° C., and the humidity is 93%;

[0081] (4) Bundling and oiling stage: The fiber tows are collected into bundles after cooling, and then oiled through an oil nozzle and a pre-network device to give the tows good lubricity and saturation, reducing friction and dispersion of the tows;

[0082] (5) Stretching stage: stretching the fiber obtained in step (4) at a stretching multiple of 1.2 times;

[0083] (6) Heating and setting stage: Heating and setting are carried out simultaneously with stretching, and the temperature of heat setting is 130°C;

[0084] Winding and forming stage: the composite fiber after being stretched and shaped is rolled into a regular-shaped coil by a winding device to obtain the composite fiber of this embodiment.

[0085] Comparative Example 1

[0086] The difference between Comparative Example 1 and Example 1 is that the structure of the composite fiber of Comparative Example 1 adopts a conventional inverted "8"-shaped parallel structure.

[0087] Comparative Example 2

[0088] The difference between Comparative Example 2 and Example 2 is that the structure of the composite fiber of Comparative Example 2 adopts a conventional inverted "8"-shaped parallel structure.

[0089] Comparative Example 3

[0090] The difference between Comparative Example 3 and Example 3 is that the structure of the composite fiber of Comparative Example 3 adopts a conventional inverted "8"-shaped parallel structure.

[0091] Comparative Example 4

[0092] A composite fiber consists of two island structure fibers and one bridge structure fiber, wherein the bridge structure fiber is high-viscosity PA6 (relative viscosity is 3.16), and the island structure fiber is low-viscosity PA6 (relative viscosity is 2.46), the relative viscosity of the high-viscosity PA6 is 0.7 higher than the relative viscosity of the low-viscosity PA6, and the mass ratio of the high-viscosity PA6 to the low-viscosity PA6 is 50:50.

[0093] The only difference between Comparative Example 4 and Example 1 is that the raw materials of the island structure fiber and the bridge structure fiber of the composite fiber of Comparative Example 4 are exchanged, and the preparation method of the composite fiber is the same as that of Example 1.

[0094] Performance Testing

[0095] The composite fiber samples prepared in Examples 1-4 and Comparative Examples 1-4 were subjected to performance tests, wherein: the mechanical properties were tested according to the standard GB / T14344-2008; the curling properties were tested according to the standard GB / T6506-2001. The test results are shown in Table 1.

[0096] Table 1: Performance comparison of composite fiber samples obtained in various embodiments and comparative examples

[0097]

[0098] As shown in Table 1, the composite fiber embodiments 1-4 of the present invention with island-bridge structure all have better mechanical properties and three-dimensional curling elasticity, among which COPA is the curling elasticity of the embodiment 4 of the island structure fiber. At the same time, the three-dimensional curling elasticity of the embodiments 1-3 is improved to a certain extent compared with the comparative examples 1-3 of the ordinary inverted "8" shaped parallel composite fibers. Since the relative viscosity of the island structure fiber of comparative example 4 is lower than the relative viscosity of the bridge structure fiber, although the mechanical properties of the composite fiber do not change much, the curling performance (curl shrinkage CC%) is greatly reduced.

[0099] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, without having to go through creative labor. Therefore, simple improvements made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the protection scope of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should belong to the protection scope of the present invention.

Claims

1. A composite fiber, It is characterized in that The composite fiber includes two island structure fibers and one bridge structure fiber, wherein the bridge structure fiber is arranged between the two island structure fibers to connect the two island structure fibers together and form a flat island bridge structure with large ends and a small middle; the island structure fibers and the bridge structure fibers are both polyamide fibers; the relative viscosity or thermal shrinkage rate of the island structure fibers is greater than that of the bridge structure fibers, the relative viscosity of the island structure fibers is 0.5-1.5 higher than that of the bridge structure fibers, and the thermal shrinkage rate of the island structure fibers is 1.5-3 times that of the bridge structure fibers.

2. The composite fiber according to claim 1, It is characterized in that The island structure fiber includes any one of PA6, PA66, PA56 and COPA; the bridge structure fiber includes PA6.

3. The composite fiber according to claim 1, It is characterized in that The mass ratio of the island structure fibers to the bridge structure fibers is 25:75 to 75:

25.

4. The composite fiber according to claim 1, It is characterized in that The length of the bridge structure fiber is 1-5 times the diameter of the island structure fiber; the width of the bridge structure fiber is 0.1-0.5 times the diameter of the island structure fiber.

5. A method for preparing a composite fiber, It is characterized in that The preparation method is used to prepare the composite fiber according to any one of claims 1 to 4, comprising the following steps: (1) melting the raw materials for preparing the island structure fiber and the raw materials for preparing the bridge structure fiber respectively, and then entering the composite spinning assembly through their respective melt pipes. The two fiber melts are respectively ejected through the spinneret holes in the spinneret and then bonded together to form composite primary fibers with an island-bridge structure; (2) The composite spun fibers are cooled, bundled, oiled, stretched, heated, shaped, and wound to obtain the composite fibers.

6. The method for preparing the composite fiber according to claim 5, It is characterized in that In step (1), the melting temperature of the island structure fibers is 260-320° C., and the melting temperature of the bridge structure fibers is 220-265° C.; and the pressure of the composite spinning assembly is 13-25 MPa.

7. The method for preparing the composite fiber according to claim 5, It is characterized in that In step (2), the cooling is performed by side blowing; the wind speed of the side blowing is 0.25-0.5 m / s, the wind temperature is 18-20° C., and the humidity is 90-95%.

8. The method for preparing the composite fiber according to claim 5, It is characterized in that In step (2), the stretching multiple is 1.2-3.0; and the heating and setting temperature is 100-180°C.

Citation Information

Patent Citations

  • Mechanically strong absorbent non-woven fibrous mats

    CN101979745A

  • Composite elastic filament core-spun yarn fabric and preparation method thereof

    CN102454004A

  • Side by side composite fiber spinneret plate, method of preparing three-dimensional crimp antibacterial fiber with spinneret plate and application of three-dimensional crimp antibacterial fiber

    CN103225118A

  • Straight-line-shaped three-difference composite fiber and preparation method thereof

    CN109853058A

  • Dried cellulose fibers, cellulose fiber-resin composite, and molded article

    CN111533954A