A polymer microsphere and its preparation based on reverse suspension polymerization method and its application
The phosphate functionalized microspheres were prepared by reverse phase suspension polymerization and chelated with Ti4+ to obtain Ti4+-polymer microspheres, which solved the complex and time-consuming problem of the preparation of immobilized metal ion affinity chromatography materials in the prior art, and realized The efficient separation and enrichment of phosphopeptides and simplify the preparation process, suitable for large-scale production.
Patent Information
- Application Number
- CN202111145344.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-09-28
AI Technical Summary
The preparation procedures for existing immobilized metal ion affinity chromatography materials are complex, time-consuming, and are not suitable for large-scale preparation, making it difficult to effectively isolate and enrich the phosphorylated proteins/polypeptides in biological samples.
The reverse phase suspension polymerization method was used to prepare phosphate-functional polymer microspheres, and Ti4+-polymer microspheres were obtained by chelating with Ti4+. They were used as adsorbents for immobilized metal ion affinity chromatography, which simplified the preparation process and improved the Separation and enrichment efficiency.
It realizes efficient separation and enrichment of phosphopeptides, simplifies the preparation process, is suitable for large-scale production, and significantly improves the accuracy and sensitivity of analysis.
Smart Images

Figure HDA0003285374380000011 
Figure HDA0003285374380000012 
Figure HDA0003285374380000021
Abstract
Description
Technical Field
[0001] The present invention relates to a Ti prepared by reverse phase suspension polymerization method. 4+ -Polymer microspheres and their application in separation and enrichment of phosphopeptides, specifically, in a dispersion medium composed of water and n-heptane, functional monomer vinylphosphonic acid and crosslinking agent N,N-methylenebisacrylamide, under the initiation of initiator sodium persulfate, are subjected to reverse suspension polymerization to obtain phosphate functionalized polymer microspheres in one step. Due to the presence of phosphate groups, the microspheres can continue to chelate Ti 4+ , two steps to get Ti 4 + -Polymer microspheres. Ti 4+ -Polymer microspheres can be directly used as adsorbents for immobilized metal ion affinity chromatography for the separation and enrichment of phosphopeptides in biological samples. Background Art
[0002] Protein phosphorylation is considered to be one of the post-translational modifications of proteins. It is involved in most life processes, such as cell division and differentiation, growth and apoptosis, and signal recognition and transmission between cells. It can also be used as a marker for abnormal expression of cancer and other diseases (Nanomaterials in Proteomics. Adv Funct Mater. N. Sun et al. 2019, 29: 1900253.). Abnormal protein phosphorylation usually leads to the occurrence of some diseases and even cancer (Magnetic metal phenolic networks: expanding the application of a promising nanoprobe to phosphoproteomics research. Che. Commun. H. Chu et al. 2020, 56: 11299-11302.). Therefore, the analysis and detection of the state and changes of phosphorylated proteins / peptides will help to further understand their mechanism of action in the body and occupy an extremely important position in the field of life sciences. At present, the "shotgun" analysis strategy is one of the main methods for phosphoproteomics research, and mass spectrometry is the most commonly used analytical tool for phosphorylated proteins / peptides (Application of tandem enrichment strategy based on MALDI_TOF_MS in phosphoproteomics. Journal of Analysis and Testing. Zhang Chuanjing et al. 2017, 36: 1064-1068.). However, due to the low content of phosphopeptides in protein hydrolysates, low ionization efficiency and interference from non-phosphorylated peptides, direct MS analysis is very difficult (Robust phosphoproteome enrichment using monodisperse microsphere-based immobilized titanium (IV) ion affinity chromatography. Nat Protoc. H. Zhou et al. 2013, 8: 461-480.). Therefore, separation and enrichment are required before analysis to improve the accuracy and sensitivity of the analysis.
[0003] So far, a variety of methods have been developed to enrich phosphorylated peptides, including immunoaffinity capture, metal oxide affinity chromatography, immobilized metal ion affinity chromatography, and ion exchange chromatography. Among them, the Ti 4+ and Zr 4+ The specific interaction between Zr and phosphorylated proteins / peptides was designed and prepared. 4+The new generation of immobilized metal ion affinity chromatography stationary phase with chelating ligand significantly improves the enrichment ability of phosphorylated proteins / peptides (Research Progress in Separation and Enrichment Methods of Phosphorylated Peptides. Journal of Analysis and Testing. Li Sha, et al. 2020, 39: 416-422, Advanced nanomaterials as sample technique for bio-analysis. TrAC-Trend AnalChem. N. Sun et al. 2021, 135: 116168.). Due to its unique selectivity and enrichment specificity for phosphorylated peptides, immobilized metal ion affinity chromatography is currently one of the most popular methods for enriching phosphorylated peptides.
[0004] At present, the main materials for immobilized metal ion affinity chromatography include nanoparticles, polymer microspheres, bulk monolithic materials and membranes, but these materials are prepared by deriving or grafting functional groups onto the matrix. For example, the immobilized metal ion affinity chromatography adsorbent prepared by Zou Hanfa's research team requires the preparation of polystyrene microspheres first, and then grafting epoxy, amino, and phosphate functional groups, and finally chelating titanium ions. After five steps of reaction, the immobilized metal ion affinity chromatography material can be obtained. The preparation procedure is complicated, the steps are numerous and time-consuming, and it is not suitable for large-scale preparation. Therefore, exploring new preparation methods with simple processes has always been a hot topic of research (Facile preparation of bifunctional adsorbents for efficiently enriching N-glycopeptides and phosphopeptides. Anal Chim Acta. R. Tang et al. 2021, 1144: 111-120.). Summary of the invention
[0005] The present invention aims to provide a Ti-based suspension polymerization method. 4+ - polymer microspheres, specifically, phosphate functionalized polymer microspheres are first prepared by inverse suspension polymerization, and then further reacted with Ti 4+ Chelation to obtain Ti 4+ -Polymer microspheres. The microspheres can be directly used as immobilized metal ion affinity chromatography adsorbents to separate and enrich phosphopeptides in biological samples.
[0006] To achieve the above purpose, you can follow the following process:
[0007] 1) Preparation of phosphate functionalized polymer microspheres: In a container, add 200-1200 mg of vinylphosphonic acid, add N,N-methylenebisacrylamide in a molar ratio of 1.5 / 1-0.4 / 1 to 1-20 mL of water to form a uniform transparent solution, and adjust the solution pH to 6-8 with 1M sodium hydroxide solution; continue to add stabilizer and n-heptane, the volume ratio of n-heptane to water is 2 / 1-8 / 1, the stabilizer includes Span 80 and Tween 80, add 300-1500 mg The mass ratio of Span 80, Tween 80 and Span 80 is 1 / 1-2 / 3, and ultrasonic mixing is performed uniformly; 50-300 mg of initiator sodium persulfate is subsequently added, and mechanical stirring is performed at a speed of 100-300 r / min for 10-40 minutes; then the temperature is increased to 60-80° C., and stirring is continued for 4-8 hours to complete the polymerization reaction; finally, the obtained microsphere material is washed 3-5 times with an ethanol / water (1 / 1-1 / 2, v / v) mixed solvent, and vacuum dried at a temperature of 60-80° C. for 8-24 hours to obtain phosphate functionalized polymer microspheres;
[0008] 2) Ti 4+ - Preparation of polymer microspheres: 1-2 g of phosphate functionalized polymer microspheres and titanium sulfate were dispersed in 10-50 mL of water at a mass ratio of 1 / 5-1 / 50, incubated at room temperature for 6-12 hours, washed the obtained material with ethanol / water (1 / 1-1 / 2, v / v) mixed solvent 3-5 times, and vacuum dried at 60-80°C for 8-24 hours to obtain Ti 4+ -Polymer microspheres.
[0009] The present invention has the following advantages:
[0010] (1) Phosphate-functionalized polymer microspheres can be obtained by a one-step reaction based on the reverse suspension polymerization method. The production process is simple, the reaction conditions are mild, and it is suitable for large-scale preparation;
[0011] (2) Phosphate-functionalized polymer microspheres do not require subsequent grafting or derivatization and can be directly bonded to Ti 4+ The chelation was carried out in two steps to obtain Ti 4+ - polymer microspheres;
[0012] (3) Ti 4+ -Polymer microspheres, used as adsorbents for immobilized metal ion affinity chromatography, have high efficiency in separation and enrichment of phosphopeptides in biological samples. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Ti 4+ -Schematic diagram of the preparation of polymer microspheres.
[0014] Figure 2 Ti 4+ - Helium ion scanning electron microscopy images of polymer microspheres. a: Example 1, b: Example 2, c: Comparative Example 2, d: Comparative Example 3.
[0015] Figure 3 Comparison of Fourier transform-infrared spectra of phosphate-functionalized polymer microspheres and their preparation monomers.
[0016] Figure 4 Ti 4+ -Full spectrum of X-ray photoelectron spectroscopy of polymer microspheres and high-resolution spectrum of Ti 2p.
[0017] Figure 5 Ti 4+ -Nitrogen adsorption / desorption curves and pore size distribution of polymer microspheres. a, c: nitrogen adsorption / desorption curves, b, d: pore size distribution.
[0018] Figure 6 Ti 4+ -Comparison of mass spectra of the mixed enzymatic solution of β-casein and bovine serum albumin (1 / 100, mass ratio) before and after enrichment by polymer microspheres. a: before enrichment, b: Ti 4+ -Polymer microspheres I enriched; c: Ti 4+ -After enrichment with polymer microsphere II. * represents phosphopeptides, # represents dephosphorylated fragments
[0019] Figure 7 Mass spectra of the mixed enzymatic hydrolysate of β-casein and bovine serum albumin (1 / 100, mass ratio) after enrichment. a: Commercial Ti 4+ -After affinity chromatography microsphere enrichment, b: Ti 4+ -After enrichment of polymer microspheres III, c:Ti 4+ -After enrichment with polymer beads IV, * represents phosphopeptides and # represents dephosphorylated fragments. DETAILED DESCRIPTION
[0020] Example 1 Ti 4+ -Preparation and application of polymer microspheres I
[0021] Ti 4+ - Preparation of polymer microspheres I:
[0022] 1) Preparation of phosphate functionalized polymer microspheres I. In a container, add 1080 mg of vinylphosphonic acid, add N,N-methylenebisacrylamide in 12 mL of water according to the molar ratio of N,N-methylenebisacrylamide to vinylphosphonic acid of 1 / 1, form a uniform transparent solution, and adjust the solution pH to 7 with 1M sodium hydroxide solution; continue to add stabilizer and n-heptane, the volume ratio of n-heptane to the aqueous phase is 5 / 1, the stabilizer includes Span 80 and Tween 80, add 1200 mg of Span 80, the mass ratio of Tween 80 to Span 80 is 2 / 3, and ultrasonic mixing is uniform; then add 200 mg of initiator sodium persulfate, mechanically stir at a speed of 300 r / min for 30 minutes; then increase the temperature to 70°C, continue stirring for 6 hours to complete the polymerization reaction; finally, wash the obtained microsphere material with ethanol / water (1 / 1, volume ratio) mixed solvent 3 times, and vacuum dry at 60°C for 12 hours to obtain phosphate functionalized polymer microspheres I;
[0023] 2) Ti 4+ -Preparation of polymer microspheres I. 1 g of polymer microspheres I containing phosphate functional groups and titanium sulfate were dispersed in 40 mL of water at a mass ratio of 1 / 10 of polymer microspheres to titanium sulfate, incubated at room temperature for 8 hours, and the obtained material was washed 5 times with a mixed solvent of ethanol / water (1 / 1, volume ratio), and vacuum dried at 60°C for 12 hours to obtain Ti 4+ -Polymer microspheres I.
[0024] Ti 4+ -Application of polymer microspheres I:
[0025] Preparation of β-casein enzymatic hydrolysate sample: Dissolve 2.0 mg of β-casein in 200 μL of a denaturant aqueous solution containing 6 M guanidine hydrochloride and 100 mM NH4HCO3. Add 1.4 mL of Tris-HCl buffer. Add trypsin at an enzyme to protein ratio of 1:25, react in a 37°C water bath for 16 h, and store in a -20°C refrigerator for later use.
[0026] Preparation of bovine serum albumin (BSA) hydrolyzate sample: Dissolve 2.0 mg of BSA in 1.0 mL of denaturant aqueous solution containing 8 M urea and 100 mM NH4HCO3. Then add 20 μL of 1 M dithiothreitol aqueous solution, centrifuge at 10000 r / min for 20 min, and keep constant temperature at 37°C for 2 h. Continue to add 7.4 mg of iodoacetamide in a light-proof state, and react in a light-proof state for 35 min. After taking it out, add 7.0 mL of Tris-HCl buffer. Add trypsin according to the enzyme to protein ratio of 1:25, react in a water bath at 37°C for 18 h, and desalt the obtained hydrolyzate, freeze-dry it, and store it in a refrigerator at -20°C for use.
[0027] Phosphorylated peptide enrichment process: First, 200 μL of loading solution (ACN / H2O / TFA, 80 / 14 / 6, v / v / v) was used to balance the Ti 4+ -polymer microspheres I twice, each time shaking at room temperature for 15 min, centrifuged, and the supernatant removed. 100 μL of loading solution containing β-casein / BSA (m / m) enzymatic hydrolyzate with a mass ratio of 1 / 100 (ACN / H2O / TFA, 80 / 14 / 6, v / v / v) and 100 μL of 0.1% TFA aqueous solution were added to Ti in a ratio of 1 / 1 (v / v). 4+ -polymer microsphere material, shake the sample at room temperature for 30 minutes, centrifuge, and remove the supernatant. Then use eluent A (ACN / H2O / TFA, 50 / 44 / 6, v / v / v) containing 400mM NaCl to elute twice (200μL×2 times), shake each time for 15 minutes, centrifuge, and remove the supernatant to remove non-phosphopeptides and other impurities. Then add eluent B (ACN / H2O / TFA, 30 / 69.9 / 0.1, v / v / v) to elute twice (200μL×2 times) to remove salt. Then add 100μL of 10% NH3.H2O eluent and shake at room temperature for 15 minutes, centrifuge, and take the supernatant for matrix-assisted laser desorption ionization time-of-flight mass spectrometry (MALDI-TOF / MS) analysis.
[0028] Product characterization
[0029] Helium ion scanning electron microscope Figure 2 As shown in a, the material is spherical with a particle size of 10 to 22 μm.
[0030] The infrared spectra of the phosphate functionalized polymer microspheres and their precursors prepared in Example 1 are as follows: Figure 3 As shown, the wave number in the spectrum of monomer vinylphosphonic acid is 1108 cm -1 , 1023cm -1The absorption peaks correspond to the stretching vibration peaks of the P=O bond and the PO bond in -PO3. These peaks appear simultaneously in the infrared spectrum of the phosphate functionalized polymer microspheres. The wave number in the spectrum of the crosslinker N,N-methylenebisacrylamide is 1655cm -1 and 1538cm -1 The absorption peaks correspond to the stretching vibration peaks of amide bond I-C=O and amide II-NH, which are also present in the infrared spectrum of phosphate-functionalized polymer microspheres. However, the stretching vibration of C=C bond (1625cm -1 ) was not observed in the spectrum of phosphate-functionalized polymer microspheres, indicating that C=C was consumed during the polymerization reaction. These analytical results indicate that phosphate-functionalized polymer microspheres were prepared from the precursors vinylphosphonic acid and N,N-methylenebisacrylamide through the ethylene free radical reaction.
[0031] Figure 4 Ti 4+ - Experimental results of the full spectrum of X-ray photoelectron spectroscopy of polymer microspheres and high-resolution spectrum of Ti 2p. In the full spectrum, Ti 4+ - The absorption peaks of C, O, P and Ti atoms in polymer microspheres ( Figure 4 a). In the Ti 2p high-resolution energy spectrum, the absorption peaks at binding energies of 458.7eV and 464.4eV correspond to the 3 / 2p and 1 / 2p orbitals of Ti, respectively ( Figure 4 b) From this we can see that Ti 4+ -Polymer microspheres are successfully bonded to Ti through phosphate groups on the surface of the microspheres 4+ Prepared by chelation.
[0032] Figure 5 The results of nitrogen physical adsorption / desorption experiments are shown in Figure 2. 4+ -The specific surface area of polymer microsphere I is 204.9 m 2 g -1 , the average pore size is 15.5nm mesoporous ( Figure 5 b).
[0033] Product Application
[0034] Ti 4+ -Polymer microspheres I can be used as an adsorbent for immobilized metal ion affinity chromatography to separate and enrich phosphopeptides in samples. Figure 6 The following is a comparison of the mass spectra of the mixed enzymatic hydrolysate of β-casein and bovine serum albumin before and after enrichment. Figure 6 As shown in a, before enrichment, the peak signals with higher intensity in the spectrum are all signal peaks of non-phosphopeptides, and the signals of phosphopeptides are almost all suppressed, and no obvious phosphopeptide signals are observed.4+ -After enrichment of polymer microspheres I, Figure 6 As shown in b, the non-phosphopeptide peaks were significantly reduced, and the phosphopeptide peak signals were significantly enhanced. Three typical phosphopeptide signal peaks (2061, 2556, 3121, m / z) and their dephosphorylated fragment peaks (1963, 2458, 3023, m / z) were detected, indicating that the Ti 4+ -Polymer microspheres I have a high enrichment effect and selectivity for phosphopeptides.
[0035] Example 2 Ti 4+ -Preparation and application of polymer microspheres II
[0036] Ti 4+ -Preparation of polymer microspheres II:
[0037] In the preparation process of phosphate functionalized polymer microspheres II, the mass of the functional monomer vinylphosphonic acid was reduced to 864 mg, and the remaining preparation conditions were the same as those in the titanium ion chelation process in Example 1. 4+ - Preparation of polymer microspheres I.
[0038] Ti 4+ - The application of polymer microspheres II is also the same as in Example 1Ti 4+ -Application of polymer microspheres I.
[0039] Product characterization
[0040] Ti 4+ - Helium ion scanning electron microscopy of polymer microspheres II Figure 2 As shown in b, the material is spherical with a particle size of 15 to 35 μm. The results of the nitrogen physical adsorption / desorption experiment ( Figure 5 a) shows that Ti 4+ -Polymer microspheres II have a higher specific surface area than Ti 4+ -Polymer microspheres I is low, with a value of 158.0m 2 g -1 The pore size distribution shows that the microspheres are 4+ -Polymer microsphere II is similar, also contains mesopores, with an average pore size of 14.2nm ( Figure 5 b). This may be because the content of the functional monomer vinylphosphonic acid decreased during the preparation of polymer microspheres-II, resulting in an increase in the relative content of the crosslinking agent N,N-methylenebisacrylamide in the reaction solution, an increase in the degree of crosslinking, and a decrease in the comparative area.
[0041] Product Application
[0042] like Figure 6 c, using Ti 4+- When polymer microsphere II was used as adsorbent, three characteristic phosphopeptides (2061, 2556, 3121, m / z) could also be enriched from the mixed enzymatic hydrolysate of β-casein and bovine serum albumin (1 / 100, mass ratio), indicating that it has good enrichment efficiency and selectivity. 4+ -Compared with the enrichment effect of polymer microspheres I, the interference of non-phosphopeptides was slightly higher, indicating that Ti 4+ -Polymer microspheres II are less selective for phosphopeptides than Ti 4+ -Polymer microspheres I. This may be due to the fact that less functional monomer vinylphosphonic acid is used in the preparation process, resulting in a decrease in the number of phosphate binding sites available after the microspheres are formed, and thus a smaller number of titanium ions can be chelated.
[0043] Comparative Example 1
[0044] Enrichment of phosphopeptides using commercially available immobilized metal ion affinity chromatography microspheres
[0045] For comparison with the examples, commercial Ti was purchased from Bailingwei Technology Co., Ltd. 4+ - affinity microsphere material (SPE-Ti-IMAC, particle size 40-100 μm), under the same conditions (same as Example 1Ti 4+ -polymer microspheres I) were used to enrich the phosphopeptides in the mixed enzymatic hydrolysate of β-casein and bovine serum albumin. The results are shown in Figure 7 Although three characteristic phosphopeptide signals can be detected (2061, 2556, 3121, m / z), and the interference of non-phosphopeptides is almost negligible, their signal intensities are significantly lower than those in Examples 1 and 2. This shows that although the commercial SPE-Ti-IMAC microspheres have good selectivity for phosphopeptides, their enrichment efficiency is slightly low.
[0046] Comparative Example 2
[0047] Ti 4+ -Preparation of polymer microspheres III:
[0048] In the preparation process of phosphate functionalized polymer microspheres III, the 1M sodium hydroxide solution was replaced with ammonia water of equal molar mass concentration, and the remaining preparation conditions were the same as those in the titanium ion chelation process in Example 1. Example 1Ti 4+ - Preparation of polymer microspheres I.
[0049] Ti 4+ - The application of polymer microspheres III is also the same as in Example 1Ti 4+ -Application of polymer microspheres I.
[0050] Product characterization
[0051] Ti 4+ - Helium ion scanning electron microscopy of polymer microspheres III Figure 2 c shows that the material is amorphous and non-spherical. The results of the nitrogen physical adsorption / desorption experiment ( Figure 5 c) shows that Ti 4+ -Polymer microspheres III have a higher specific surface area than Ti 4+ -Polymer microspheres I and II are both low, with values of 11.6 m 2 g -1 The pore size distribution shows that the material is a mesoporous material with an average pore size of 5.9 nm ( Figure 5 d) This may be because it does not form a ball, is amorphous and has a low yield. 4+ - Half of the polymer microspheres I and II cannot form a cross-linked structure, resulting in almost no specific area.
[0052] Product Application
[0053] like Figure 7 As shown in b, using Ti 4+ - When polymer microspheres III were used as adsorbents, three characteristic phosphopeptides (2061, 2556, 3121, m / z) could also be enriched from the mixed enzymatic hydrolysate of β-casein and bovine serum albumin (1 / 100, mass ratio), indicating that it has an enrichment effect on phosphopeptides. 4+ Compared with the enrichment effect of polymer microspheres I and II, there is more interference from non-phosphopeptides and the signal intensity is lower, indicating that Ti 4+ -Polymer microspheres III are less selective and less efficient in enriching phosphopeptides than Ti 4+ -Polymer microspheres I. This may be due to their amorphous morphology, almost no specific surface area, and few phosphate binding sites, so the number of titanium ions that can be chelated is small.
[0054] Comparative Example 3
[0055] Ti 4+ -Preparation of polymer microspheres IV:
[0056] In the preparation process of phosphate functionalized polymer microspheres IV, the 1M sodium hydroxide solution was directly replaced with a titanium sulfate solution of equimolar mass concentration without the step of chelating titanium ions. The remaining preparation conditions were the same as those in Example 1. Example 1Ti 4+ - Preparation of polymer microspheres I.
[0057] Ti 4+ - The application of polymer microspheres IV is also the same as in Example 1Ti 4+ -Application of polymer microspheres I.
[0058] Product characterization
[0059] Ti 4+ - Helium ion scanning electron microscopy of polymer microspheres IV Figure 2 As shown in d, the material is amorphous and non-spherical. The results of the nitrogen physical adsorption / desorption experiment ( Figure 5 c) shows that Ti 4+ -Polymer microspheres IV have a higher specific surface area than Ti 4+ -Polymer microspheres I and II are both low, with values of 12.1m 2 g -1 , same as Ti 4+ - polymer microspheres III, and have almost no specific surface area. Its pore size distribution shows that it contains mesopores, with an average pore size of 6.8nm ( Figure 5 d) This may be because directly adding titanium sulfate into the solution does not form microspheres, and the yield is the same as Ti 4+ -Polymer microspheres III are equivalent and cannot form a cross-linked structure, resulting in almost no specific area.
[0060] Product Application
[0061] like Figure 7 c, using Ti 4+ - When polymer microspheres IV were used as adsorbents, only two characteristic phosphopeptides (2061, 3121, m / z) could be enriched from the mixed enzymatic hydrolysate of β-casein and bovine serum albumin (1 / 100, mass ratio), indicating that its enrichment efficiency for phosphopeptides was low. 4+ Compared with the enrichment effect of polymer microspheres I, there is a lot of interference from non-phosphopeptides. The signal intensity of non-phosphopeptides has suppressed the signal intensity of phosphopeptides, so the signal intensity of phosphopeptides is less than 1000, indicating that Ti 4+ -Polymer microspheres IV are less selective and less efficient in enriching phosphopeptides than Ti 4+ -Polymer microspheres I. This may be due to their amorphous morphology, almost no specific surface area, and few phosphate binding sites, so the number of titanium ions that can be chelated is small.
[0062] The above results show that the Ti prepared by the present invention 4+ -Polymer microspheres I showed high enrichment efficiency and selectivity for phosphopeptides. The preparation method adopted is simple to operate. Phosphate-functionalized polymer microspheres can be synthesized in one step by reverse suspension polymerization and can be directly combined with Ti without secondary modification. 4 Chelation to prepare Ti for enrichment of phosphopeptides 4 + -Polymer microspheres greatly simplify the preparation process and are suitable for large-scale preparation.
Claims
1. A method for preparing polymer microspheres based on inverse suspension polymerization, wherein vinylphosphonic acid VPA is used as a functional monomer, N,N-methylenebisacrylamide MBA is used as a crosslinker, an oil-in-water system is formed in the presence of a stabilizer, and inverse suspension polymerization is used to prepare phosphate-functionalized polymer microspheres in one step through a free radical polymerization reaction; the microspheres are further reacted with titanium ions (Ti 4+ ) for chelation to obtain Ti for phosphopeptide enrichment 4+ - polymer microspheres; Ti 4+ -Polymer microspheres were prepared as follows: 1) Preparation of phosphate functionalized polymer microspheres: In a container, add 200-1200 mg of vinylphosphonic acid, add N,N-methylenebisacrylamide in a molar ratio of 1.5 / 1-0.4 / 1 to 1-20 mL of water to form a uniform transparent solution, and adjust the solution pH to 6-8 with 1 M sodium hydroxide solution; continue to add stabilizer and n-heptane, the volume ratio of n-heptane to the aqueous phase is 2 / 1-8 / 1, the stabilizer includes Span 80 and Tween 80, add 300-1500 mg of Span 80, the mass ratio of Tween 80 to Span 80 is 1 / 1-2 / 3, and mix evenly by ultrasonication; then add 50-300 mg of initiator sodium persulfate, and mechanically stir at a speed of 100-300 r / min for 10-40 min. min; then the temperature is raised to 60-80°C and the stirring is continued for 4-8 hours to complete the polymerization reaction; finally, the obtained microsphere material is washed 3-5 times with a mixed solvent of ethanol / water 1 / 1-1 / 2, v / v, and vacuum dried at a temperature of 60-80°C for 8-24 hours to obtain phosphate functionalized polymer microspheres; 2) Ti 4+ - Preparation of polymer microspheres: 1-2 g of phosphate-functionalized polymer microspheres and titanium sulfate were dispersed in 10-50 mL of water at a mass ratio of 1 / 5-1 / 50, incubated at room temperature for 6-12 hours, washed 3-5 times with a mixed solvent of ethanol / water (1 / 1-1 / 2, v / v), and dried in vacuum at 60-80°C for 8-24 hours to obtain Ti 4+ -Polymer microspheres.
2. A polymer microsphere prepared by the method of claim 1.
3. An application of the polymer microspheres according to claim 2, characterized in that: The microspheres can be used as an adsorbent or stationary phase for immobilized metal ion affinity chromatography and can be used for separation and enrichment of phosphopeptides in biological samples.
4. The use according to claim 3, characterized in that: The biological sample is one or more of human and / or animal body fluids, tissue enzymatic hydrolysate and cell enzymatic hydrolysate.
Citation Information
Patent Citations
Immobilized metal ion affinity chromatography microsphere material as well as preparation and application thereof
CN113351190A
Immobilized titanium ion affinity chromatography material and its preparation and application
US20090101581A1
Method for enriching phosphopeptides
US20100273984A1