A titanium dioxide phosphate compound and its preparation method and application
By forming a three-dimensional network structure in the titanium dioxide phosphate compound, the problem of low efficiency of anatase-type titanium dioxide in visible light is solved, and efficient catalytic reaction and adsorption capacity under low or no light conditions is achieved, and the preparation cost is reduced.
Patent Information
- Application Number
- CN202211638477.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-19
AI Technical Summary
The existing anatase-type titanium dioxide photocatalysts have low efficiency under visible light, and the existing phosphorylated TiO2 preparation methods are costly and have large particles, making it difficult to effectively utilize light energy.
By dropwise adding a mixed liquid of a titanium source and an alcohol solvent to the phosphoric acid solution, combining silicate and acidic solution for heating treatment, a titanium dioxide phosphate compound with a high specific surface area is prepared, forming a titanium octahedral and phosphooxygen four-sided surface of titanium octahedral and phosphooxygen The body is bound by a three-dimensional network structure with oxygen bridges, breaking the ordered structure and improving photocatalytic performance.
It realizes efficient catalytic reaction under low light or no light conditions, removes harmful gases in air and wastewater, has excellent photocatalytic degradation and adsorption capabilities, is low in cost, and is suitable for large-scale production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium dioxide modification, and in particular to a titanium dioxide phosphate compound and a preparation method and application thereof. Background Art
[0002] When exposed to light, nano-titanium dioxide will generate electrons and holes, which react with water or oxygen adsorbed around it to generate superoxide radicals. The superoxide radicals have extremely strong oxidative decomposition ability, which can kill bacteria and decompose organic pollutants. The photocatalyst composed of rutile titanium dioxide can be used for antibacterial tiles, self-cleaning building materials, super-hydrophilic materials, deodorization / deodorization materials, water purification, cancer treatment, etc. However, rutile carbon dioxide requires ultraviolet rays below 400nm for excitation; sunlight and artificial light that can become excitation light sources contain much more visible light than ultraviolet rays. However, the photocatalyst composed of the above-mentioned titanium dioxide cannot make good use of visible light. From the perspective of energy conversion efficiency, the efficiency of rutile titanium dioxide is very low.
[0003] As a type of TiO2, phosphorylated TiO2 is structurally different from the ordered structure of TiO2. Due to the addition of P element, the originally ordered structure of TiO2 becomes disordered to a certain extent, resulting in an increase in its specific surface area. Therefore, phosphorylated TiO2 has different properties from crystalline TiO2. Phosphorylated TiO2 has broad application prospects in the preparation of solar cells, photocatalysts, and adsorbents. Although the solid-phase sintering method for preparing phosphorylated TiO2 is simple, the particles are large, agglomeration is serious, the cost is high, and a phase transition occurs above a certain temperature (600°C).
[0004] Therefore, it is of great significance to obtain a method for preparing a titanium dioxide phosphate compound with low cost, high specific surface area and good photocatalytic performance. Summary of the invention
[0005] The purpose of the present invention is to provide a titanium dioxide phosphate compound and a preparation method and application thereof in view of the deficiencies in the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a titanium dioxide phosphate compound, comprising the following steps:
[0008] 1) adding a mixture of a titanium source and an alcohol solvent dropwise into a phosphoric acid solution to obtain a titanium phosphate solution;
[0009] 2) mixing a titanium phosphate solution and a silicate to obtain a mixed solution; the mixed solution and an acidic solution are then mixed and then subjected to heating and drying treatments to obtain a titanium dioxide phosphate compound;
[0010] The dripping rate of step 1) is 0.5-1.5 mL / min.
[0011] Preferably, the titanium source in step 1) comprises one or more of tetrabutyl titanate, titanium tetraisopropoxide and tetraethyl titanate; and the alcohol solvent is ethanol, butanol or isopropanol.
[0012] Preferably, in step 1), the volume ratio of the titanium source to the alcohol solvent is 1:25-55; the volume ratio of the titanium source to the phosphoric acid solution is 1:20-50, and the mass concentration of the phosphoric acid solution is 0.1-0.8%.
[0013] Preferably, in step 2), the mass ratio of the titanium phosphate solution to the silicate is 100:0.2-0.8, and the volume ratio of the titanium phosphate solution to the acidic solution is 100:1-3.
[0014] Preferably, the mass concentration of the acidic solution in step 2) is 25-35%, and the acidic solution is hydrochloric acid, sulfuric acid or nitric acid.
[0015] Preferably, in step 2), the mixed solution is allowed to stand and then mixed with the acidic solution; the standing time is 1 to 2 hours; the heating temperature is 85 to 95° C., and the heating time is 0.5 to 1.5 hours.
[0016] The present invention also provides a titanium dioxide phosphate compound prepared by the preparation method, wherein the specific surface area of the titanium dioxide phosphate compound is 290 to 330 m 2 / g.
[0017] The invention also provides application of the titanium dioxide phosphate compound in photocatalyst and adsorbent.
[0018] The beneficial effects of the present invention include the following:
[0019] 1) The titanium dioxide phosphate compound of the present invention has strong adsorption and potential transfer of nanoparticle characteristics, produces high-energy metathesis reaction, can produce catalytic reaction under weak light or even no light conditions, can significantly and permanently remove harmful gases such as formaldehyde, benzene, ammonia in the air, and has antibacterial, mildew-proof and air-purifying effects; has a large specific surface area and strong adsorption capacity, can efficiently remove organic pollutants in wastewater, and silicate plays the role of bonding and stabilizing the solution. The method of the present invention is simple in process, low in cost, and suitable for large-scale production.
[0020] 2) In the present invention, a mixture of a titanium source and an alcohol solution is added dropwise to a phosphoric acid solution. The titanium source exists in the alcohol solvent in the form of Ti-OH, and the phosphoric acid exists in water in the form of HPO4 2- and Ti-OH and HPO4 2- , Combined and dehydrated, a three-dimensional network structure is formed by the titanium oxygen octahedron (titanium is an octahedral structure) and the phosphorus oxygen tetrahedron (phosphorus is a tetrahedral structure) connected by oxygen bridges. Due to the presence of the phosphorus oxygen tetrahedron, the original orderly octahedral structure is broken, causing a certain degree of disorder in the crystalline titanium dioxide. In addition, Ti-OH and HPO4 2- , Combination and dehydration will create holes and increase its specific surface area. DETAILED DESCRIPTION
[0021] The present invention provides a method for preparing a titanium dioxide phosphate compound, comprising the following steps:
[0022] 1) adding a mixture of a titanium source and an alcohol solvent dropwise into a phosphoric acid solution to obtain a titanium phosphate solution;
[0023] 2) mixing a titanium phosphate solution and a silicate to obtain a mixed solution; the mixed solution and an acidic solution are then mixed and then subjected to heating and drying treatments to obtain a titanium dioxide phosphate compound;
[0024] The dripping rate of step 1) is 0.5-1.5 mL / min.
[0025] In the present invention, the titanium source in step 1) preferably comprises one or more of tetrabutyl titanate, titanium tetraisopropoxide and tetraethyl titanate; and the alcohol solvent is preferably ethanol, butanol or isopropanol.
[0026] In the present invention, the volume ratio of the titanium source and the alcohol solvent in step 1) is preferably 1:25-55, more preferably 1:30-50, and more preferably 1:35-45.
[0027] In the present invention, the volume ratio of the titanium source and the phosphoric acid solution in step 1) is preferably 1:20-50, more preferably 1:25-45, and more preferably 1:30-40; the mass concentration of the phosphoric acid solution is preferably 0.1-0.8%, more preferably 0.2-0.7%, and more preferably 0.3-0.6%; the phosphoric acid solution is an aqueous phosphoric acid solution.
[0028] In the present invention, the rate of the dropping in step 1) is preferably 0.7 to 1.3 mL / min, more preferably 0.9 to 1.1 mL / min, and more preferably 1 mL / min; during the dropping process, the temperature of the phosphoric acid solution is preferably 60 to 80°C, more preferably 65 to 75°C, and more preferably 70°C.
[0029] In the present invention, the mass ratio of the titanium phosphate solution and the silicate in step 2) is preferably 100:0.2-0.8, more preferably 100:0.3-0.7, and more preferably 100:0.4-0.6; the silicate is preferably sodium silicate or potassium silicate; the volume ratio of the titanium phosphate solution and the acidic solution is preferably 100:1-3, more preferably 100:1.5-2.5, and more preferably 100:2.
[0030] In the present invention, the mass concentration of the acidic solution in step 2) is preferably 25-35%, more preferably 27-32%, and more preferably 29-31%; the acidic solution is preferably hydrochloric acid, sulfuric acid or nitric acid.
[0031] In step 2) of the present invention, the mixed solution is preferably allowed to stand before mixing with the acidic solution; the standing time is preferably 1 to 2 hours, more preferably 1.5 hours; the heating temperature is preferably 85 to 95°C, more preferably 88 to 92°C, more preferably 90°C; the heating time is preferably 0.5 to 1.5 hours, more preferably 0.8 to 1.2 hours, more preferably 1 hour.
[0032] The present invention also provides a titanium dioxide phosphate compound prepared by the preparation method, wherein the specific surface area of the titanium dioxide phosphate compound is 290 to 330 m 2 / g.
[0033] The invention also provides application of the titanium dioxide phosphate compound in photocatalyst and adsorbent.
[0034] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0035] Example 1
[0036] 10 mL of tetrabutyl titanate was added to 280 mL of ethanol to obtain a mixed solution; phosphoric acid and water were mixed to obtain a phosphoric acid solution with a mass concentration of 0.2%. 250 mL of phosphoric acid solution was heated to 62°C and kept constant, and the mixed solution of tetrabutyl titanate and ethanol was added dropwise to the phosphoric acid solution at a rate of 0.8 mL / min to obtain a titanium phosphate solution.
[0037] Sodium silicate is added to a titanium phosphate solution (the mass ratio of sodium silicate to the titanium phosphate solution is 0.3:100) to obtain a uniform mixed solution. The mixed solution is allowed to stand at room temperature for 1 hour and then mixed with sulfuric acid having a mass concentration of 28% (the mass ratio of sulfuric acid to the titanium phosphate solution is 1.5:100), heated at 85°C for 1 hour and then dried at 50°C to obtain a titanium dioxide phosphate compound.
[0038] The specific surface area of the titanium dioxide phosphate compound in this example is 295 m 2 / g, has excellent photocatalytic degradation and adsorption capabilities, good stability and durability, and has good catalytic activity in both ultraviolet and visible light ranges.
[0039] Example 2
[0040] 10 mL of titanium tetraisopropoxide was added to 500 mL of butanol to obtain a mixed solution; phosphoric acid and water were mixed to obtain a phosphoric acid solution with a mass concentration of 0.8%. 450 mL of phosphoric acid solution was heated to 75°C and kept constant, and the mixed solution of titanium tetraisopropoxide and butanol was added dropwise to the phosphoric acid solution at a rate of 1.2 mL / min to obtain a titanium phosphate solution.
[0041] Potassium silicate is added to a titanium phosphate solution (the mass ratio of potassium silicate to the titanium phosphate solution is 0.7:100) to obtain a uniform mixed solution. The mixed solution is allowed to stand at room temperature for 2 hours and then mixed with nitric acid having a mass concentration of 33% (the mass ratio of nitric acid to the titanium phosphate solution is 2.5:100), heated at 93°C for 0.5 hours and then dried at 45°C to obtain a titanium dioxide phosphate compound.
[0042] The specific surface area of the titanium dioxide phosphate compound in this example is 310 m 2 / g, has excellent photocatalytic degradation and adsorption capabilities, good stability and durability, and has good catalytic activity in both ultraviolet and visible light ranges.
[0043] Example 3
[0044] 10 mL of tetraethyl titanate was added to 400 mL of isopropanol to obtain a mixed solution; phosphoric acid and water were mixed to obtain a phosphoric acid solution with a mass concentration of 0.5%. 350 mL of phosphoric acid solution was heated to 70°C and kept constant, and the mixed solution of tetraethyl titanate and isopropanol was added dropwise to the phosphoric acid solution at a rate of 1 mL / min to obtain a titanium phosphate solution.
[0045] Potassium silicate is added to a titanium phosphate solution (the mass ratio of potassium silicate to the titanium phosphate solution is 0.5:100) to obtain a uniform mixed solution. The mixed solution is allowed to stand at room temperature for 1.5 hours and then mixed with hydrochloric acid having a mass concentration of 30% (the mass ratio of hydrochloric acid to the titanium phosphate solution is 2:100), heated at 90°C for 1 hour and then dried at 48°C to obtain a titanium dioxide phosphate compound.
[0046] The specific surface area of the titanium dioxide phosphate compound in this example is 325 m 2 / g, has excellent photocatalytic degradation and adsorption capabilities, good stability and durability, and has good catalytic activity in both ultraviolet and visible light ranges.
[0047] Comparative Example 1
[0048] The volume of isopropanol in Example 3 was changed to 700 mL, the heating temperature of the phosphoric acid solution was changed to 40° C., the dropping rate of the mixed solution of tetraethyl titanate and isopropanol was changed to 2 mL / min, and the other conditions were the same as in Example 3.
[0049] The specific surface area of the titanium dioxide phosphate compound in this comparative example is 240 m 2 / g.
[0050] Comparative Example 2
[0051] The potassium silicate in Example 3 was omitted, and the titanium phosphate solution and the hydrochloric acid solution were directly mixed. The volume of the phosphoric acid solution was changed to 150 mL, and the heating temperature was changed from 90° C. to 70° C. The other conditions were the same as in Example 3.
[0052] The specific surface area of the titanium dioxide phosphate compound in this comparative example is 255 m 2 / g.
[0053] Take 20 mg of the titanium dioxide phosphate compounds of Examples 1 to 3 and Comparative Examples 1 to 2 respectively, and add them to 50 mL of 10 -4 mol / L Rhodamine B solution, the light source is a 500W halogen tungsten lamp, and a filter is used to ensure that the incident light is visible light. A sample is taken every 8 minutes, and after centrifugation, the supernatant is measured using an ultraviolet spectrophotometer, and the concentration change of Rhodamine B during the photocatalytic degradation process is determined based on the absorbance value at 554nm.
[0054] The degradation rate of the compound of Example 1 to Rhodamine B was 98% when irradiated with light for 40 minutes, and the degradation was complete in 48 minutes; the degradation rate of the compound of Example 2 to Rhodamine B was 99% when irradiated with light for 40 minutes, and the degradation was complete in 48 minutes; the compound of Example 3 completely degraded Rhodamine B when irradiated with light for 40 minutes. The degradation rate of the compound of Comparative Example 1 to Rhodamine B was 90% when irradiated with light for 40 minutes, and the degradation rate was 93% when irradiated with light for 48 minutes; the degradation rate of the compound of Comparative Example 2 to Rhodamine B was 92% when irradiated with light for 40 minutes, and the degradation rate was 94% when irradiated with light for 48 minutes.
[0055] After the titanium dioxide phosphate compounds obtained in the three embodiments of the present invention photocatalyzed Rhodamine B, the titanium dioxide phosphate compounds were cleaned and dried, and then Rhodamine B was photocatalytically degraded under the same conditions as above, which was repeated 5 times. After each degradation was completed, the titanium dioxide phosphate compounds were cleaned and dried; in the fifth photocatalysis, the degradation rate of Rhodamine B by the compound of the present invention reached more than 97% when illuminated for 40 minutes, and had good stability and durability.
[0056] The titanium dioxide phosphate compound of the present invention can produce a catalytic reaction under weak light or even no light conditions, and can significantly and permanently remove harmful gases such as formaldehyde, benzene, ammonia, etc. in the air, and has the effects of antibacterial, mildew-proof, and air purification; it has a large specific surface area and strong adsorption capacity, and can efficiently remove organic pollutants in wastewater.
[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Application of a titanium dioxide phosphate compound in photocatalytic degradation of rhodamine B, characterized in that: The preparation method of the titanium dioxide phosphate compound comprises the following steps: 1) adding a mixture of a titanium source and an alcohol solvent dropwise into a phosphoric acid solution to obtain a titanium phosphate solution; 2) mixing a titanium phosphate solution and a silicate to obtain a mixed solution; the mixed solution and an acidic solution are then mixed and then subjected to heating and drying treatments to obtain a titanium dioxide phosphate compound; Step 1) The rate of the dropping is 0.5-1.5 mL / min; during the dropping process, the temperature of the phosphoric acid solution is 60-70° C.; Step 1) The volume ratio of the titanium source to the alcohol solvent is 1:25-55; the volume ratio of the titanium source to the phosphoric acid solution is 1:20-50, and the mass concentration of the phosphoric acid solution is 0.1-0.8%; Step 2) the mass ratio of the titanium phosphate solution to the silicate is 100:0.2-0.8, and the volume ratio of the titanium phosphate solution to the acidic solution is 100:1-3; The temperature of the heating treatment is 85 to 95° C., and the time of the heating treatment is 0.5 to 1.5 h.
2. The use according to claim 1, characterized in that: Step 1) The titanium source comprises one or more of tetrabutyl titanate, titanium tetraisopropoxide and tetraethyl titanate; and the alcohol solvent is ethanol, butanol or isopropanol.
3. The use according to claim 1, characterized in that: Step 2) The mass concentration of the acidic solution is 25-35%, and the acidic solution is hydrochloric acid, sulfuric acid or nitric acid.
4. The use according to claim 1 or 3, characterized in that: In step 2), the mixed solution is allowed to stand for 1 to 2 hours before being mixed with the acidic solution.